A Comparison of Stress Corrosion Cracking Susceptibility in Additively-Manufactured and Wrought Materials for Aerospace and Biomedical Applications
Michael Roach1, R. Scott Williamson1, Jonathan Pegues2,3, Nima Shamsaei2,3,* 1Department of Biomedical Materials Science, University of Mississippi Medical Center,
Jackson, MS 39216 2Department of Mechanical Engineering, Auburn University, Auburn, AL 36849
3National Center for Additive Manufacturing Excellence (NCAME), Auburn University, Auburn, AL 36849
*Corresponding author: shamsaei@auburn.edu
Abstract
Additive manufacturing (AM) is becoming an increasingly popular method in both aerospace and biomedical industries. Titanium alloys are increasingly common in additive manufactured applications due to their excellent strength to weight ratio and biocompatibility. Traditional wrought Ti-6Al-4V alloys show little sensitivity to stress corrosion cracking (SCC) when subjected to in-vitro conditions. In AM applications the alloy powder is often sifted and reused multiple times which often results in a degradation of the powder’s shape. Recent studies have also shown that the oxygen content of additive powders increases with repeated powder use which may increase the susceptibility of the resulting parts to SCC. This research compares the microstructural characteristics and tensile SCC behavior of AM Ti-6Al-4V parts fabricated from new and recycled powder in distilled H2O, salt water, and Ringers solution. Additionally, the effect of surface finish is investigated for each microstructure comparing the as-built surfaces to machined and polished surfaces.
Keywords: Stress corrosion cracking, environmentally assisted cracking, titanium alloy, tensile properties
Introduction
As additively manufacturing becomes a more viable option for fabrication of structural components in a wide range of biomedical and aerospace applications there is a critical need to understand the failure mechanisms related to these specific applications. As a result, numerous studies have recently been published comparing mechanical behavior of additively manufactured (AM) titanium alloy parts to their wrought material counterparts [1]–[13]. Despite this recent surge
1410
Solid Freeform Fabrication 2018: Proceedings of the 29th Annual InternationalSolid Freeform Fabrication Symposium – An Additive Manufacturing Conference
mailto:shamsaei@auburn.edu
of research the effect of environmentally assisted cracking (EAC) and its effect of stress corrosion cracking (SCC) has not been well represented for additive manufactured (AM) materials.
Titanium alloys such as Ti-6Al-4V are common in both biomedical and aerospace industries due to their high strength to weight ratio, biocompatibility, and excellent corrosion resistance. In both of these industries parts are often subjected to harsh environments that may lead to an increased susceptibility to SCC [14], [15]. While the EAC failure mechanisms are well reported for wrought Ti-6Al-4V and believed to be of relatively low risk, however, the unique microstructure, equilibrium phases, and high surface roughness associated with AM parts could lead to an increased risk of SCC compared to its wrought counterpart. Recent studies have also shown that the oxygen content of additive powders increases with repeated powder use which may increase the susceptibility of the resulting parts to SCC [16], [17].
The purpose of the present research was to compare the ASTM G129 slow strain rate (SSR) SCC susceptibility of Ti-6Al-4V samples fabricated using laser powder bed fusion (LPBF) technology, to those fabricated using traditional machined wrought samples from the same alloy. The ductility of AM Ti-6Al-4V samples were compared to their wrought counterparts in distilled water, Ringer’s, and 3.5% NaCl electrolytes. Additionally, the SCC response of titanium AM samples fabricated from the virgin and reconditioned powders were compared for both as-built and machined conditions.
Experimental Set-up
Test coupons were designed accordance to ASTM G129 [18] with the dimensions shown in Figure 1. Grip ends were threaded in order to submerge the test coupons in the desired solution during testing. Two solutions, Ringer’s and 3.5% NaCl, were selected to test for stress corrosion cracking susceptibility compared to distilled H2O as the control solution. Ringer’s solution is often used in testing to simulate physiological conditions. Additionally, a 3.5% NaCl solution is often used in testing to simulate a seawater environment. For the Ringer’s solution, a test temperature of 37°C was chosen as a representative in-vivo condition for surgical implants while room temperature (23°C) was selected for testing in the 3.5% NaCl solution. For the control solution, a test temperature of 37°C was used.
1411
Figure 1: Specimen geometry used for slow strain rate testing.
Slow strain rate tensile tests were performed on an MTS load frame with a 100 kN capacity. A displacement stroke rate of 2.5x10-5 mm/s was chosen which results in an approximate strain rate of 1x10-6 s-1. Test specimens were completely submerged in the test solution and the temperature was monitored and controlled using a Digi-Sense temperature controller. Figure 2 gives a representation of the test setup used for this study. All samples were tested until failure, after which, a measuring microscope was used to determine the elongation to failure and reduction of area (RoA). Fracture surfaces were then examined with both a Keyence digital microscope and a Zeiss scanning electron microscope (SEM). Ratios between the control environment and the harsh environment were calculated by dividing the mean values of samples in harsh environments by the mean values of the samples in the control (distilled H2O). ASTM G129 [18] states that ratios that are less than unity are considered to be susceptible to SCC. For this study a more strict definition of ratios falling below 0.9, which has been used in previous studies [14], is considered to be susceptible to SCC.
1412
Figure 2: Test set up showing specimen submerged in solution during testing.
Results
The elongation to failure, reduction of area, and time to failure were averaged for each condition and are listed in Table 1. The elongation and reduction of area are significantly lower than the wrought conditions which is consistent with literature on L-PBF Ti-6Al-4V [5], [13], [19]. The low ductility of AM L-PBF Ti-6Al-4V is attributed to the fine acicular martensitic microstructure as a result of the high cooling rate during fabrication. Rapid solidification in the fabrication process does not allow the diffusive a transformation to occur, thus, the β phase transforms to the α’ phase through the non-diffusive martensitic transformation [20]. Additionally, the elongation to failure for all conditions reported in this study is much lower than the required 10% elongation to failure required by ASTM F2924 [21] for AM Ti-6Al-4V.
Table 1: Slow strain rate results for each condition.
Condition Powder Solution Temp. (°C)
Elongation (%)
RoA (%)
Time (Hrs)
As-Built New H2O 37 6.27 28.2 41.29
As-Built Reused H2O 37 6.10 25.2 40.15
1413
As-Built New Ringers 37 5.58 23.3 40.79
As-Built Reused Ringers 37 5.31 25.2 39.93
As-Built New 3.5% NaCl 23 5.30 21.7 38.33
As-Built Reused 3.5% NaCl 23 4.97 23.9 38.16
Machined New H2O 37 5.92 31.9 39.12
Machined New Ringers 37 5.83 34.0 41.01
Wrought [1] NA H2O 37 21.8 53.7 NA
Wrought [1] NA Ringers 37 20.5 53.3 NA
A visual representation of the slow strain rate tensile properties for each condition is shown using a box plot in Figure 3. The dotted lines on each box plot represents the lower range of the control solution with the black line representing the machined control condition and the red line representing the as-built control condition. The elongation to failure was mostly similar for all conditions and solutions with only the 3.5% NaCl solution showing significant decreases. There was a slight decrease in elongation to failure for samples in Ringer’s, however, the difference is not significant. A similar trend was observed for the reduction of area (RoA) with Ringer’s and 3.5% NaCl showing slightly lower RoA. Interestingly, while no difference was observed between as-built and machined specimens in elongation to failure, as-built specimens did show consistent decreases in RoA compared to machined specimens. Finally, there was no significant differences in the time to failure for all conditions.
1414
Figure 3: Box plots showing the spread in data for all conditions.
Evaluation of environmentally assisted cracking for slow strain rate testing, according to ASTM G129 [18], is carried out by comparing the SSR ratios to the control environment with ratios reaching unity being considered not susceptible to SCC. Decreasing SSR ratios are considered to show increasing susceptibility to SCC. In general, for biomedical applications, ratios that are lower than 0.9 are considered to show some susceptibility to SCC [14]. Table 2 lists the elongation ratio (RE), the reduction of area ratio (RRA), and time to failure ratio (RTTF) calculated
1415
for each condition. The control for all machined specimens is the machined new powder in distilled H20 while the control for all as-built conditions was the as-built new powder in distilled H20.
Table 2: Calculated ratios for each condition, * represents control for surface condition.
Condition Powder Solution Temp. (°C) RE RRA RTTF
*Machined New H2O 37 1.00 1.00 1.00
Machined New Ringers 37 0.98 1.07 1.05
Machined New 3.5% NaCl 23 0.87 0.93 0.97
*As-Built New H2O 37 1.00 1.00 1.00
As-Built Reused H2O 37 0.97 0.89 0.97
As-Built New Ringers 37 0.89 0.83 0.99
As-Built Reused Ringers 37 0.85 0.90 0.97
As-Built New 3.5% NaCl 23 0.84 0.77 0.93
As-Built Reused 3.5% NaCl 23 0.79 0.85 0.92
Comparing the ratios for each condition given in Table 2, there are several areas that indicate susceptibility to SCC for L-PBF Ti-6Al-4V. For the machined conditions there is a decrease in the elongation to failure in the 3.5% NaCl solution, however, the reduction of area is only slightly reduced. The most notable observation is the significant decrease in ductility for all as-built conditions. While the elongation to failure ratio was not significantly reduced for distilled H2O fabricated from both new and reused powder, all other as-built geometries showed significant (< 0.9) decreases in RE. Additionally, the RRA was also considered to be significant (< 0.9) for all as-built surfaces outside of the control condition. This indicates that the high roughness associated with the as-built geometries could potentially increase the susceptibility of EAC for AM Ti-6Al-4V. Additionally, all 3.5% NaCl environments showed some loss in ductility compared to the control environment with significantly low RRA (≤ 0.75) for the as-built conditions. The reduced ductility for the Ringer’s and 3.5% NaCl conditions suggests that AM Ti-6Al-4V parts could potentially show an increased risk of EAC in harsh environments in the presence of high surface roughness. Additionally, another observation than can be made from Table 2 is the further decrease in ductility for all 3.5% NaCl solutions. More tests for specimens in 3.5% NaCl at 37° C and distilled H2O at 23°C are necessary to ensure the difference in testing temperature is not playing some role in the SCC behavior.
Fractography analysis revealed a change in crack behavior between the control and 3.5% NaCl solutions while the Ringer’s solution was mostly similar to the control. Representative fracture surfaces for each condition are shown in Figure 4. For the control condition in Fig. 4(a) the crack propagation appears to be deflect along prior β grains as indicated by the deep valleys. Closer inspection of these valleys to the right of Fig. 4(a) reveals that these appear to be ends of
1416
prior β grains being pulled completely from the surface. This type of crack propagation results in multiple crack deflections leading to a tortuous fracture surface. Similarly, the fracture surface of the representative Ringer’s solution in Fig. 4(b) shows multiple crack deflections along the prior β grains resulting in a tortuous fracture surface. Conversely, the 3.5% NaCl fracture surface shows a less tortuous crack path which is attributed to very little failure along prior β grains. This type of crack propagation consists of less crack deflection ultimately leading to the lower ductility in the 3.5% NaCl specimens.
0
Figure 4: Fracture surfaces of the as-built condition in a) distilled H2O, b) Ringers, and c) 3.5% NaCl.
1417
Conclusions
The results presented in this study indicate that additive manufactured Ti-6Al-4V may be susceptible to stress corrosion cracking. A decrease in elongation to failure was observed for a solution of machined 3.5% NaCl while the machined Ringer’s solution showed similar elongation to failure as the control in the machined condition. However, all samples in the as-built condition showed significant reduction of area ratios (< 0.9) compared to the as-built control. The reduction in elongation to failure in the as-built conditions was observable but less severe than the reduction of area. This significant loss in ductility for the as-built specimens in Ringer’s and 3.5% NaCl compared to distilled H2O in the as-built condition indicate that the presence of the rough surface may increase the susceptibility of AM Ti-6Al-4V to SCC. These results, while preliminary, do indicate that stress corrosion cracking could be of concern for AM Ti-6Al-4V in the presence of harsh environments. Further tests are in progress to determine the effect of testing temperature in relation to the test solution. Additionally, further in-depth studies are needed to fully assess the effect of harsh environments on AM parts.
Acknowledgements
Partial funding for this work was provided by the National Science Foundation under Grant No. 1657195. Supports from the Naval Air Systems Command (NAVAIR) is also greatly appreciated.
References
[1] B. E. Carroll, T. A. Palmer, and A. M. Beese, “Anisotropic tensile behavior of Ti–6Al–4Vcomponents fabricated with directed energy deposition additive manufacturing,” Acta Mater., vol. 87,no. Supplement C, pp. 309–320, Apr. 2015.
[2] A. J. Sterling, B. Torries, N. Shamsaei, S. M. Thompson, and D. W. Seely, “Fatigue behavior andfailure mechanisms of direct laser deposited Ti–6Al–4V,” Mater. Sci. Eng. A, vol. 655, pp. 100–112,Feb. 2016.
[3] K. S. Chan, M. Koike, R. L. Mason, and T. Okabe, “Fatigue Life of Titanium Alloys Fabricated byAdditive Layer Manufacturing Techniques for Dental Implants,” Metall. Mater. Trans. A, vol. 44, no.2, pp. 1010–1022, Feb. 2013.
[4] P. Edwards and M. Ramulu, “Fatigue performance evaluation of selective laser melted Ti–6Al–4V,”Mater. Sci. Eng. A, vol. 598, pp. 327–337, Mar. 2014.
[5] L. Facchini, E. Magalini, P. Robotti, A. Molinari, S. Höges, and K. Wissenbach, “Ductility of a Ti‐6Al‐4V alloy produced by selective laser melting of prealloyed powders,” Rapid Prototyp. J., vol. 16,no. 6, pp. 450–459, Oct. 2010.
[6] D. A. Hollander et al., “Structural, mechanical and in vitro characterization of individually structuredTi–6Al–4V produced by direct laser forming,” Biomaterials, vol. 27, no. 7, pp. 955–963, Mar. 2006.
[7] M. Kahlin, H. Ansell, and J. J. Moverare, “Fatigue behaviour of additive manufactured Ti6Al4V, withas-built surfaces, exposed to variable amplitude loading,” Int. J. Fatigue, vol. 103, pp. 353–362, Oct.2017.
1418
[8] S. Leuders et al., “On the mechanical behaviour of titanium alloy TiAl6V4 manufactured by selectivelaser melting: Fatigue resistance and crack growth performance,” Int. J. Fatigue, vol. 48, pp. 300–307, Mar. 2013.
[9] H. Matsumoto et al., “Room-temperature ductility of Ti–6Al–4V alloy with α′ martensitemicrostructure,” Mater. Sci. Eng. A, vol. 528, no. 3, pp. 1512–1520, Jan. 2011.
[10] L. E. Murr et al., “Microstructures and mechanical properties of electron beam-rapid manufacturedTi–6Al–4V biomedical prototypes compared to wrought Ti–6Al–4V,” Mater. Charact., vol. 60, no.2, pp. 96–105, Feb. 2009.
[11] R. K. Nalla, R. O. Ritchie, B. L. Boyce, J. P. Campbell, and J. O. Peters, “Influence of microstructureon high-cycle fatigue of Ti-6Al-4V: Bimodal vs. lamellar structures,” Metall. Mater. Trans. A, vol.33, no. 3, pp. 899–918, Mar. 2002.
[12] J. Pegues, M. Roach, R. Williamson, and N. Shamsaei, “Surface Roughness Effects on the FatigueStrength of Additively Manufactured Ti-6Al-4V,” Int. J. Fatigue, Accepted 2018.
[13] W. Xu et al., “Additive manufacturing of strong and ductile Ti–6Al–4V by selective laser melting viain situ martensite decomposition,” Acta Mater., vol. 85, no. Supplement C, pp. 74–84, Feb. 2015.
[14] R. S. Williamson, M. D. Roach, and L. D. Zardiackas, “Comparison of Stress Corrosion Cracking ofTi-15Mo, Ti-6Al-7Nb, Ti-6Al-4V, and CP Ti,” ASTM Int. STP, vol. 1471, pp. 166–177, 2004.
[15] M. D. Roach, R. S. Williamson, and L. D. Zardiackas, “Comparison of the Corrosion FatigueCharacteristics of CP Ti-Grade 4, Ti-6AI-4V ELI, Ti-6AI-7Nb, and Ti-15Mo,” ASTM Int., Jan. 2006.
[16] J. C. Fox, S. P. Moylan, and B. M. Lane, “Effect of Process Parameters on the Surface Roughness ofOverhanging Structures in Laser Powder Bed Fusion Additive Manufacturing,” Procedia CIRP, vol.45, pp. 131–134, Jan. 2016.
[17] Y. Sun, M. Aindow, and R. J. Hebert, “The effect of recycling on the oxygen distribution in Ti-6Al-4V powder for additive manufacturing,” Mater. High Temp., vol. 35, no. 1–3, pp. 217–224, May2018.
[18] “Standard Practice for Slow Strain Rate Testing to Evaluate the Susceptibility of Metallic Materialsto Environmentally Assisted Cracking,” 2013.
[19] J. Pegues et al., “Effect of Process Parameter Variation on Microstructure and Mechanical Propertiesof Additively Manufactured Ti-6Al-4V,” Solid Free. Fabr. 2017 Proc. 28th Annu. Int., p. 14, 2017.
[20] J. Yang, H. Yu, J. Yin, M. Gao, Z. Wang, and X. Zeng, “Formation and control of martensite in Ti-6Al-4V alloy produced by selective laser melting,” Mater. Des., vol. 108, pp. 308–318, Oct. 2016.
[21] “Standard Specification for Additive Manufacturing Titanium-6 Aluminum-4 Vanadium withPowder Bed Fusion,” 14.
1419
WelcomeTitle PagePrefaceOrganizing CommitteePapers to JournalsTable of ContentsBroader ImpactsUsing Additive Manufacturing as a Pathway to Change the Qualification ParadigmTechnology Integration into Existing CompaniesLattice Design Optimization: Crowdsourcing Ideas in the ClassroomEducation of Additive Manufacturing – An Attempt to Inspire ResearchPrinting Orientation and How Implicit It IsMethod for a Software-Based Design Check of Additively Manufactured ComponentsThe Recycling of E-Waste ABS Plastics by Melt Extrusion and 3D Printing Using Solar Powered Devices as a Transformative Tool for Humanitarian Aid
Binder JettingEvaluating the Surface Finish of A356-T6 Cast Parts from Additively Manufactured Sand MoldsEconomies of Complexity of 3D Printed Sand Molds for CastingMitigating Distortion During Sintering of Binder Jet Printed CeramicsBinder Jetting of High Temperature and Thermally Conductive (Aluminum Nitride) CeramicBinder Jetting Additive Manufacturing of Water-Atomized Iron
Data Analytics in AMEffects of Thermal Camera Resolution on Feature Extraction in Selective Laser MeltingArtificial Intelligence-Enhanced Multi-Material Form Measurement for Additive MaterialsMachine Learning for Modeling of Printing Speed in Continuous Projection StereolithographyCurvature-Based Segmentation of Powder Bed Point Clouds for In-Process MonitoringNondestructive Micro-CT Inspection of Additive Parts: How to Beat the BottlenecksNon-Destructive Characterization of Additively Manufactured Components Using X-Ray Micro-Computed TomographyPrecision Enhancement of 3D Printing via In Situ MetrologyLayer-Wise Profile Monitoring of Laser-Based Additive ManufacturingCorrelative Beam Path and Pore Defect Space Analysis for Modulated Powder Bed Laser Fusion Process
Hybrid AMCharacterization of High-Deposition Polymer Extrusion in Hybrid ManufacturingMechanical Properties Evaluation of Ti-6Al-4V Thin-Wall Structure Produced by a Hybrid Manufacturing ProcessDevelopment of Pre-Repair Machining Strategies for Laser-Aided Metallic Component RemanufacturingViscosity Control of Pseudoplastic Polymer Mixtures for Applications in Additive ManufacturingCuring Behavior of Thermosets for the Use in a Combined Selective Laser Sintering Process of PolymersEffect of Porosity on Electrical Insulation and Heat Dissipation of Fused Deposition Modeling Parts Containing Embedded WireA New Digitally Driven Process for the Fabrication of Integrated Flex-Rigid ElectronicsHybrid Manufacturing with FDM Technology for Enabling Power Electronics Component FabricationDigitally-Driven Micro Surface Patterning by Hybrid ManufacturingPotentials and Challenges of Multi-Material Processing by Laser-Based Powder Bed FusionA Digitally Driven Hybrid Manufacturing Process for the Flexible Production of Engineering Ceramic ComponentsStereolithography-Based Manufacturing of Molds for Directionally Solidified CastingsExamination of the Connection between Selective Laser-Melted Components Made of 316L Steel Powder on Conventionally Fabricated Base BodiesCharacterization and Analysis of Geometric Features for the Wire-Arc Additive Process
ApplicationsGeometry/Surface FinishEffect of Inter-Layer Cooling Time on Distortion and Mechanical Properties in Metal Additive ManufacturingEffect of Shield Gas on Surface Finish of Laser Powder Bed Produced PartsMaterial Characterization for Lightweight Thin Wall Structures Using Laser Powder Bed Fusion Additive ManufacturingMetal Additive Manufacturing in the Oil and Gas IndustryDevelopment of a Customized CPAP Mask Using Reverse Engineering and Additive Manufacturing
Specific PartsMultimaterial Aerosol Jet Printing of Passive Circuit ElementsAdditive Manufacturing of Liners for Shaped ChargesAn Aerospace Integrated Component Application Based on Selective Laser Melting: Design, Fabrication and Fe SimulationAdditive Manufacturing of Metal Bandpass Filters for Future Radar ReceiversFast Prediction of Thermal History in Large-Scale Parts Fabricated via a Laser Metal Deposition ProcessDesign Guidelines for a Software-Supported Adaptation of Additively Manufactured Components with Regard to a Robust Production
Large Scale PartsIncreasing Interlaminar Strength in Large Scale Additive ManufacturingUsing Post-Tensioning in Large Scale Additive Parts for Load Bearing StructuresPrecast Concrete Molds Fabricated with Big Area Additive Manufacturing3D Printed Fastener-Free Connections for Non-Structural and Structural Applications – An Exploratory InvestigationCorrelations of Interlayer Time with Distortion of Large Ti-6Al-4V Components in Laser Metal Deposition with WireModel Development for Residual Stress Consideration in Design for Laser Metal 3D Printing of Maraging Steel 300Topology Optimisation of Additively Manufactured Lattice Beams for Three-Point Bending Test
Residual StressMorphable Components Topology Optimization for Additive ManufacturingNext-Generation Fibre-Reinforced Lightweight Structures for Additive Manufacturing
Topology OptimizationTopology Optimized Heat Transfer Using the Example of an Electronic HousingMicrostructural and Mechanical Characterization of Ti6Al4V Cellular Struts Fabricated by Electron Beam Powder Bed Fusion Additive ManufacturingEffect of Wall Thickness and Build Quality on the Compressive Properties of 304L Thin-Walled Structure Fabricated by SLMMechanical Behavior of Additively Manufactured 17-4 Ph Stainless Steel Schoen Gyroid Lattice Structure
Lattices and CellularAn Investigation of the Fatigue Strength of Multiple Cellular Structures Fabricated by Electron Beam Powder Bed Fusion Additive Manufacturing ProcessOn the Mechanical Behavior of Additively Manufactured Asymmetric HoneycombsFabrication of Support-Less Engineered Lattice Structures via Jetting of Molten Aluminum DropletsFinite Element Modeling of Metal Lattice Using Commercial Fea PlatformsA CAD-Based Workflow and Mechanical Characterization for Additive Manufacturing of Tailored Lattice StructuresA Comparison of Modeling Methods for Predicting the Elastic-Plastic Response of Additively Manufactured Honeycomb StructuresNumerical and Experimental Study of the Effect of Artificial Porosity in a Lattice Structure Manufactured by Laser Based Powder Bed FusionSize and Topology Effects on Fracture Behavior of Cellular StructuresRheological, In Situ Printability and Cell Viability Analysis of Hydrogels for Muscle Tissue RegenerationDevelopment of a Thermoplastic Biocomposite for 3D PrintingDesign Rules for Additively Manufactured Wrist Splints Created Using Design of Experiment Methods
Biomedical ApplicationsDesign and Additive Manufacturing of a Patient Specific Polymer Thumb Splint ConceptMandibular Repositioning Appliance following Resection Crossing the Midline- A3D Printed GuideA Sustainable Additive Approach for the Achievement of Tunable PorosityEffects of Electric Field on Selective Laser Sintering of Yttria-Stabilized Zirconia Ceramic PowderFabrication of Ceramic Parts Using a Digital Light Projection System and Tape CastingSlurry-Based Laser Sintering of Alumina CeramicsMaterial Properties of Ceramic Slurries for Applications in Additive Manufacturing Using Stereolithography
MaterialsCeramicsAdditive Manufacturing of Alumina Components by Extrusion of In-Situ UV-Cured PastesMechanical Challenges of 3D Printing Ceramics Using Digital Light ProcessingEffect of Laser Additive Manufacturing on Microstructure Evolution of Inoculated Zr₄₅ꓸ₁Cu₄₅ꓸ₅Al5Co₂ Bulk Metallic Glass Matrix CompositesFiber-Fed Printing of Free-Form Free-Standing Glass StructuresAdditive Manufacturing of Energetic MaterialsMethods of Depositing Anti-Reflective Coatings for Additively Manufactured OpticsA Review on the Additive Manufacturing of Fiber Reinforced Polymer Matrix Composites
Non-Traditional Non-MetalsDesign and Robotic Fabrication of 3D Printed Moulds for CompositesMechanical Property Correlation and Laser Parameter Development for the Selective Laser Sintering of Carbon Fiber Reinforced Polyetheretherketone4D Printing Method Based on the Composites with Embedded Continuous FibersFabricating Functionally Graded Materials by Ceramic On-Demand Extrusion with Dynamic Mixing
CompositesThe Effect of Shear-Induced Fiber Alignment on Viscosity for 3D Printing of Reinforced PolymersProcessing Short Fiber Reinforced Polymers in the Fused Deposition Modeling ProcessImpact Testing of 3D Printed Kevlar-Reinforced Onyx MaterialDeposition Controlled Magnetic Alignment in Iron-PLA CompositesEffects of In-Situ Compaction and UV-Curing on the Performance of Glass Fiber-Reinforced Polymer Composite Cured Layer by LayerGeneral Rules for Pre-Process Planning in Powder Bed Fusion System – A ReviewDevelopment of an Engineering Diagram for Additively Manufactured Austenitic Stainless Steel AlloysFatigue Life Prediction of Additively Manufactured Metallic Materials Using a Fracture Mechanics ApproachCharacterizing Interfacial Bonds in Hybrid Metal Am Structures
Direct WriteThe Mechanical Behavior of AISI H13 Hot-Work Tool Steel Processed by Selective Laser Melting under Tensile Stress
Broad IssuesAdditive Manufacturing of Metal Functionally Graded Materials: A ReviewUnderstanding Adopting Selective Laser Melting of Metallic MaterialsThe Effect of Processing Parameter on Zirconium Modified Al-Cu-Mg Alloys Fabricated by Selective Laser MeltingSelective Laser Melting of Al6061 Alloy: Processing, Microstructure, and Mechanical PropertiesSmall-Scale Characterization of Additively Manufactured Aluminum Alloys through Depth-Sensing IndentationEffects of Process Parameters and Heat Treatment on the Microstructure and Mechanical Properties of Selective Laser Melted Inconel 718Effects of Design Parameters on Thermal History and Mechanical Behavior of Additively Manufactured 17-4 PH Stainless Steel
AluminumThe Effects of Powder Recycling on the Mechanical Properties of Additively Manufactured 17-4 PH Stainless SteelMechanical Properties of 17-4 Ph Stainless Steel Additively Manufactured Under Ar and N₂ Shielding GasRecyclability of 304L Stainless Steel in the Selective Laser Melting ProcessThe Influence of Build Parameters on the Compressive Properties of Selective Laser Melted 304L Stainless Steel
NickelCharacterization of Impact Toughness of 304L Stainless Steel Fabricated through Laser Powder Bed Fusion Process
17-4PH Stainless SteelIncorporation of Automated Ball Indentation Methodology for Studying Powder Bed Fabricated 304L Stainless SteelEffect of Powder Degradation on the Fatigue Behavior of Additively Manufactured As-Built Ti-6Al-4VVolume Effects on the Fatigue Behavior of Additively Manufactured Ti-6Al-4V Parts
304 Stainless SteelEffects of Layer Orientation on the Multiaxial Fatigue Behavior of Additively Manufactured Ti-6Al-4VAmbient-Temperature Indentation Creep of an Additively Manufactured Ti-6Al-4V AlloyIndividual and Coupled Contributions of Laser Power and Scanning Speed towards Process-Induced Porosity in Selective Laser MeltingA Comparison of Stress Corrosion Cracking Susceptibility in Additively-Manufactured and Wrought Materials forAerospace and Biomedical Applications
316L Stainless SteelEffect of Energy Density on the Consolidation Mechanism and Microstructural Evolution of Laser Cladded Functionally-Graded Composite Ti-Al System
TitaniumMechanical Properties of Zr-Based Bulk Metallic Glass Parts Fabricated by Laser-Foil-Printing Additive ManufacturingExperimental Characterization of Direct Metal Deposited Cobalt-Based Alloy on Tool Steel for Component RepairPEEK High Performance Fused Deposition Modeling Manufacturing with Laser In-Situ Heat TreatmentA Comparative Investigation of Sintering Methods for Polymer 3D Printing Using Selective Separation Shaping (SSS)Not Just Nylon... Improving the Range of Materials for High Speed SinteringMaterial Property Changes in Custom-Designed Digital Composite Structures Due to Voxel SizeQuantifying the Effect of Embedded Component Orientation on Flexural Properties in Additively Manufactured Structures
Non-Traditional MetalsInfluences of Printing Parameters on Semi-Crystalline Microstructure of Fused Filament Fabrication Polyvinylidene Fluoride (PVDF) ComponentsEffects of Build Parameters on the Mechanical and Di-Electrical Properties of AM Parts
Novel PolymersLaser Sintering of PA12/PA4,6 Polymer CompositesUnderstanding Hatch-Dependent Part Properties in SLSInvestigation into the Crystalline Structure and Sub-Tₚₘ Exotherm of Selective Laser Sintered Polyamide 6The Influence of Contour Scanning Parameters and Strategy on Selective Laser Sintering PA613 Build Part PropertiesProcessing of High Performance Fluoropolymers by Laser Sintering
Polymers for Material ExtrusionReinforcement Learning for Generating Toolpaths in Additive ManufacturingControl System Framework for Using G-Code-Based 3D Printing Paths on a Multi-Degree of Freedom Robotic ArmAnalysis of Build Direction in Deposition-Based Additive Manufacturing of Overhang Structures
Polymers for Powder Bed FusionTopology-Aware Routing of Electric Wires in FDM-Printed ObjectsUsing Autoencoded Voxel Patterns to Predict Part Mass, Required Support Material, and Build TimeContinuous Property Gradation for Multi-Material 3D-Printed ObjectsConvection Heat Transfer Coefficients for Laser Powder Bed FusionLocal Thermal Conductivity Mapping of Selective Laser Melted 316L Stainless Steel
ModelingFinite Element Modeling of the Selective Laser Melting Process for Ti-6Al-4VModelling the Melt Pool of the Laser Sintered Ti6Al4V Layers with Goldak’S Double-Ellipsoidal Heat SourceA Novel Microstructure Simulation Model for Direct Energy Deposition ProcessInfluence of Grain Size and Shape on Mechanical Properties of Metal Am MaterialsExperimental Calibration of Nanoparticle Sintering SimulationSolidification Simulation of Direct Energy Deposition Process by Multi-Phase Field Method Coupled with Thermal Analysis
Physical ModelingThermal Modeling Power BedsEstablishing Property-Performance Relationships through Efficient Thermal Simulation of the Laser-Powder Bed Fusion ProcessAn Investigation into Metallic Powder Thermal Conductivity in Laser Powder-Bed Fusion Additive ManufacturingSimulation of the Thermal Behavior and Analysis of Solidification Process during Selective Laser Melting of AluminaLow Cost Numerical Modeling of Material Jetting-Based Additive ManufacturingScrew Swirling Effects on Fiber Orientation Distribution in Large-Scale Polymer Composite Additive Manufacturing
Multi/Micro-Scale ModelingNumerical Prediction of the Porosity of Parts Fabricated with Fused Deposition ModelingNumerical Modeling of the Material Deposition and Contouring Precision in Fused Deposition ModelingEffect of Environmental Variables on Ti-64 Am Simulation Results
Advanced Thermal ModelingNon-Equilibrium Phase Field Model Using Thermodynamics Data Estimated by Machine Learning for Additive Manufacturing SolidificationMulti-Physics Modeling of Single Track Scanning in Selective Laser Melting: Powder Compaction EffectTowards an Open-Source, Preprocessing Framework for Simulating Material Deposition for a Directed Energy Deposition ProcessQuantifying Uncertainty in Laser Powder Bed Fusion Additive Manufacturing Models and Simulations
Modeling Part PerformanceOptimization of Inert Gas Flow inside Laser Powder-Bed Fusion Chamber with Computational Fluid DynamicsAn Improved Vat Photopolymerization Cure Model Demonstrates Photobleaching EffectsNonlinear and Linearized Gray Box Models of Direct-Write Printing DynamicsInsights into Powder Flow Characterization Methods for Directed Energy Distribution Additive Manufacturing SystemsEffect of Spray-Based Printing Parameters on Cementitious Material Distribution
Modeling InnovationsAligning Material Extrusion Direction with Mechanical Stress via 5-Axis Tool PathsFieldable Platform for Large-Scale Deposition of Concrete StructuresMicroextrusion Based 3D Printing–A Review
ImprovementsTheory and Methodology for High-Performance Material-Extrusion Additive Manufacturing under the Guidance of Force-FlowKnowledge-Based Material Production in the Additive Manufacturing Lifecycle of Fused Deposition ModelingAcoustic Emission Technique for Online Detection of Fusion Defects for Single Tracks during Metal Laser Powder Bed FusionDevelopment of an Acoustic Process Monitoring System for the Selective Laser Melting (SLM)
Process DevelopmentDepositionLow Cost, High Speed Stereovision for Spatter Tracking in Laser Powder Bed FusionMultiple Collaborative Printing Heads in FDM: The Issues in Process PlanningAdditive Manufacturing with Modular Support StructuresPick and Place Robotic Actuator for Big Area Additive Manufacturing
Extrusion3D Printed ElectronicsFiber Traction Printing--A Novel Additive Manufacturing Process of Continuous Fiber Reinforced Metal Matrix CompositeImmiscible-Interface Assisted Direct Metal Drawing
ImagingIn-Situ Optical Emission Spectroscopy during SLM of 304L Stainless SteelTool-Path Generation for Hybrid Additive ManufacturingStructural Health Monitoring of 3D Printed StructuresMechanical Properties of Additively Manufactured Polymer Samples Using a Piezo Controlled Injection Molding Unit and Fused Filament Fabrication Compared with a Conventional Injection Molding ProcessUse of SWIR Imaging to Monitor Layer-To-Layer Part Quality During SLM of 304L Stainless Steel
Novel MethodsDMP Monitoring as a Process Optimization Tool for Direct Metal Printing (DMP) of Ti-6Al-4VEffects of Identical Parts on a Common Build Plate on the Modal Analysis of SLM Created MetalOn the Influence of Thermal Lensing During Selective Laser MeltingDevelopment of Novel High Temperature Laser Powder Bed Fusion System for the Processing of Crack-Susceptible AlloysTowards High Build Rates: Combining Different Layer Thicknesses within One Part in Selective Laser MeltingLaser Heated Electron Beam Gun Optimization to Improve Additive ManufacturingTwo-Dimensional Characterization of Window Contamination in Selective Laser SinteringLaser Metal Additive Manufacturing on Graphite
Non-Metal Powder Bed FusionPredictive Iterative Learning Control with Data-Driven Model for Optimal Laser Power in Selective Laser SinteringRealtime Control-Oriented Modeling and Disturbance Parameterization for Smart and Reliable Powder Bed Fusion Additive ManufacturingMicrowave Assisted Selective Laser Melting of Technical CeramicsResearch on Relationship between Depth of Fusion and Process Parameters in Low-Temperature Laser Sintering ProcessFrequency Response Inspection of Additively Manufactured Parts for Defect IdentificationNanoparticle Bed Deposition by Slot Die Coating for Microscale Selective Laser Sintering Applications
Spinning/Pinning/StereolithographyFabrication of Aligned Nanofibers along Z-Axis – A Novel 3D Electrospinning TechniqueZ-Pinning Approach for Reducing Mechanical Anisotropy of 3D Printed PartsStructurally Intelligent 3D Layer Generation for Active-Z PrintingmicroCLIP Ceramic High-Resolution Fabrication and Dimensional Accuracy Requirements
AttendeesAuthor IndexPrintSearch