transcript
2
As per ISO 11357-1 DSC is a technique in which the difference
between the heat flow rate into a sample crucible and that into a
reference crucible is derived as a function of temperature and/or
time. During such measurement, sample and reference are subjected
to the same controlled temperature program and a specified atmos-
phere.
The heat-flux cell of DSC 214 Polyma
measuring cell
protective gas
purge gas
reference sample
Working with DSC (Differential Scanning Calorimetry) involves not
only the handling of a device, but also sample preparation,
evaluation and interpretation of the resulting curves.The DSC 214
Polyma is a key part of this concept. It provides everything a user
needs in polymer analysis.
Melting temperatures and enthalpies (heats of fusion)
Crystallization temperatures and enthalpies Glass transition
temperatures Oxidative-induction time (OIT) and oxidative-onset
temperature (OOT)
Method Differential Scanning Calorimetry
Thermal Characteristics Which Can Typically Be Detected by Using
DSC
3
Important Standards for Polymer Testing
There are several relevant standards existing for application,
evaluation and interpretation of DSC data in the polymer field. The
DSC 214 Polyma operates based on all of them. A selection of
standards can be found in the following table.
Category Standard Description
General
ISO 11357, Part 1 to 7 Plastics – Differential Scanning Calorimetry
(DSC)
ASTM D3417 Heats of Fusion and Crystallization of Polymers by
Thermal Analysis
ASTM D3418 Transition Temperatures and Enthalpy of Fusion and
Crystallization by DSC
ASTM D4591 Temperatures and Heats of Transitions of Fluoropolymers
by DSC
ASTM E793 Heats of Fusion and Crystallization by DSC
ASTM E794 Melting and Crystallization Temperatures by Thermal
Analysis
ASTM E1356 Glass Transition Temperatures by DSC
ASTM F2625 Enthalpy of Fusion, Percent Crystallinity, and Melting
Point of Ultra-High Molecular Weight Polyethylene by DSC
DIN 51007 Thermal Analysis; Differential Thermal Analysis;
Principles
DIN 53545 Bestimmung des Kälteverhaltens von Elastomeren –
Grundlagen und Prüfverfahren
EN 61074 (IEC 1074) Heats and Temperatures of Melting and
Crystallization by DSC of Electrical Insulation Materials
IEC 1006 Glass Transition Temperature of Electrical Insulation
Materials
Oxidative Stability (OIT)
ASTM D3895 Polyolefins by DSC − Oxidative-Induction Time
DS 2131.2 Pipes, Fittings and Joints of Polyethylene-Type − PEM and
PEH for Buried Gas Pipelines
DIN EN 728 Polyolefins Pipes and Fittings − Oxidative-Induction
Time
Resins/Curing
ISO 11409 Phenolic Resins − Heats and Temperatures of Reaction by
DSC
DIN 65467 Luft- und Raumfahrt: Prüfung von Reaktionsharzsystemen
mit und ohne Verstärkung, DSC-Verfahren
44
More Than a DSC – A Smart System for Polymers
Low-Mass Furnace for Fast Heating and Cooling Better Replicates
Polymer Processing Conditions The DSC 214 Polyma is equipped with
the Arena® furnace, the fastest furnace available for a heat- flux
DSC. It can heat at up to 500 K/min and cool at 200 K/min over a
wide measurement range. This even allows for the measurement of
isothermal crystallization or isothermal curing for kinetic studies
where it is necessary to reach equilibrium conditions as quickly as
possible. It is thus possible to replicate real processing
conditions very closely in your DSC experiments. Additionally, one
can speed up the measurements and thus save working time.
Unique Sensor Concept for Excellent Reproducibility
The Corona® sensor and the Concavus® pans apply the concept of a
ring-shaped contact zone which is always clearly defined. The
concave form of the pan bottom prevents it from bulging. Influences
to heat transfer are thus negligible, resulting in optimized
reproducibility. The high-grade Concavus® pans are delivered in
3in1 Trays from which they can be individually withdrawn. This
increases their mechanical stability and has an additional positive
effect on the reproducibility of the measurement results.
DSC 214 Polyma
Save Space in Your Lab
Laboratory space is often limited. With its small footprint, the
DSC 214 Polyma including cooling accessory (e.g., intracooler) is
ideally suited for this case. Its flexibility allows for easy setup
in a production environment for QA/QC purposes.
5
Proteus® Software – Setting the Paradigm in Usability and
Intelligence
SmartMode, AutoEvaluation and Identify are the keys to making life
in a laboratory much easier than ever before. Respectively, these
are: A simplified and intuitively designed user interface;
autonomous evaluation routines which can serve as a second opinion
when assessing unknown samples; and a database system for
identifying and verifying materials – all at your side at any
time. AutoCalibration performs calibration runs along the way and
keeps your hands free for more important matters.
6
The User Comes First The NETZSCH Proteus® software offers far more
than ordinary measurement and analysis software for DSC
instruments. Its many support features greatly assist operators in
their day-to-day work. But users have full control at all times and
can decide whether to go the traditional route, the software- aided
route or a combination of the two.
SmartMode and ExpertMode – Giving You the Flexibility You
Need
SW-Features
(see next pages) Identify (see next pages) TM-DSC
(temperature-
modulated DSC) ASC (Automatic Sample
Changer) support Specific heat capacity (cp) determination Report
Generator Purity Peak Separation Thermokinetics
included optional
Proteus® Software ALWAYS ONE STEP AHEAD
Due to rapid development in electronics, the timelines of embedded
display formats are often quite short. By using SmartMode, however,
it is possible to have the same intuitive user interface on a
tablet, a larger touch monitor or a regular PC – whatever you
prefer.
For anyone who favors a more classical user interface or wants
access to the entire range of functions afforded by the Proteus®
software, ExpertMode is the solution.
Real-time operation of the software allows for the display of
running curves in both modes and – if desired – presents the
evaluation immediately when the measurement is finished. In order
to start a test run, one may open either wizards (quick-start
routines in SmartMode), predefined methods (e.g., related to
polymer types in SmartMode) or user-defined methods (in both
SmartMode and ExpertMode).
SmartMode interface during an ASC measurement
7
Ideal Flat Baselines Thanks to Advanced BeFlat® Due to material and
technical limitations, each DSC sensor has some imbalances which
will have an impact on the shape of the corresponding DSC
baseline.
Advanced BeFlat® is a method to compensate all these influences in
a DSC 214 Polyma by performing just two measurements (one with a
pan only on the reference side and a second one with two empty
pans). The result are horizontal DSC baselines with minimal
deviations in the μW range.
Instrument-Independent Measurement Definitions User-defined methods
can also be stored on a network drive, acces- sible from all
existing NETZSCH DSCs with appropriate configura- tion.
Temperature- Modulated DSC – TM-DSC In TM-DSC (optional), the
under- lying linear heating rate is super- imposed by a sinusoidal
tempe- rature variation. The benefit of this procedure is the
chance to separate overlapped DSC effects by calculating the
reversing and the non-reversing signals. The reversing heat flow is
related to the changes in specific heat capacity (→ glass
transition) while the non-reversing heat flow corresponds to
temperature- dependent phenomena such as curing, dehydration or
relaxation.
Report Generator to Meet Various Needs Based on a Microsoft Word
plug-in each operator can easily create his own report template –
including logos, tables, description fields and plots. As an entry
several report examples are already delivered together with the
Proteus® software.
8
Just like Magic
AutoEvaluation AutoEvaluation is the first self-acting evaluation
routine for DSC curves on the market. Without user-intervention it
is able to detect and to evaluate fully automatic glass transition
temperatures, melting temperatures or melting enthalpies of unknown
polymers or pure metals. Experi- enced users can take the automatic
evaluation result as a second opinion – and, of course, recalculate
values if desired.
User-independent!
No evaluation macro, no selection of evaluation limits or
thresholds!
9
The Curve Comparison Database
Identify Identify is a unique software package within the thermal
analysis field for the identification and classi- fication of
materials via database comparison. Besides one-on-one comparisons
with individual curves or literature data, it also checks if a
particular curve belongs to a certain class are feasible. These
classes can consist of curves of the same material type (material
identification) but also of reference curves for Pass/Fail testing
(quality control).
The provided NETZSCH libraries contain more than 1100 entries
related to different application areas such as polymers, organics,
inorganics, metals/alloys or ceramics. The additionally available
KIMW database includes DSC curves of 600 commecially available
polymer types.
The shown similarity hit list is the result of applying Identify to
the measurement example displayed above. The highest similarity is
attributed to PA12 (polyamide 12). The similarity value of 99.5%
reflects the excellent conformity with the reference curve
(pink).
Identify Is a unique curve recognition and interpretation
system
Includes a database with NETZSCH libraries and libraries that can
be created by the user
Manages measurements, literature data and classes
10
NEW IDEAS TO GET STARTED
The SampleCutter − Perfect for Polymers One prerequisite for
reproducible and reliable DSC results is to have good thermal
contact between the sample and pan bottom, which postulates a flat
sample area. With the SampleCutter, it is easy and comfortable to
cut plane sample faces, irrespective of whether the polymer sample
is soft, hard or brittle.
Sample Preparation Kit
In addition to the SampleCutter, the DSC 214 Polyma also comes with
a Sample Preparation Kit. This set contains a variety of small
tools including a cutting board, scissors, tweezers, spatula, etc.
and is designed to make sample prepa- ration as easy and convenient
as possible.
Accessories
Concavus® Pans
The unique geometry of this sample pan features a concave bottom.
In combination with a flat sensor, it provides a ring-shaped
contact zone that is always clearly defined and accounts for
excellent reproducibility.
The New Benchmark in Sensor Design
11
3in1 Tray − The Clever Solution for Transport, Sampling and
Archiving
Even the transport and storage of the Concavus® pans is consistent
with their premium quality, thanks to the 3in1 Tray: 96 pans and
lids are packaged in an anti- static box divided into 96 separate
compartments. This elaborate packing prevents deformation of the
pans while allowing easy access to them and providing a fully
functional archiving system. The integrated sample register
including name and mass makes it easy to locate retained samples.
The Concavus® pans are actually also compatible with common
heat-flux DSCs.
Thanks to the automatic sample changer (ASC), the measurement of up
to 20 samples − either belonging to a single series or independent
of each other − can be carried out without operator intervention.
Different crucible types, different gas atmospheres and individual
calibration curves can be handled within the same carousel
run.
Automatic Sample Changer – High Sample Throughput
Liquid nitrogen cooling system (-170°C to 600°C)
Closed-loop intracooler IC40 (-40°C to 600°C)
Compressed air cooling (RT to 600°C)
Closed-loop intracooler IC70 (-70°C to 600°C)
For fast cooling back to room temperature or for tests at
sub-ambient temperatures, optimized cooling is required. NETZSCH
offers several options for meeting these needs.
Broad Temperature Range and Economic Cooling
12
Old batch
New batch
205.8 °C
244.0 °C
Glass Transition: Mid: 63.2 °C Delta Cp*: 0.064 J/(gK)
Glass Transition: Mid: 53.9 °C Delta Cp*: 0.075 J/(gK)
Partial Area: 41.57 J/g 151.2 °C ... 212.3 °C 26.3 % 151.2 °C ...
265.9 °C 100.0 %
Area: 43.62 J/g
166.2°C 167.1°C
Air
Incoming Goods Inspection
The plot shows the DSC results for two seemingly identical
granulate batches, specified as Polyamide 66, which were delivered
at different times (2nd heating after controlled cooling at 20
K/min). The blue curve (old batch) shows the glass transition at
63°C (mid-point) and the melting peak at 263°C, which are both
typical for PA66. The new batch (red curve), however, exhibits a
double peak with peak temperatures at 206°C and 244°C. This
indicates that the new granulate most probably contains a second
polymer which blends with PA66. Comparison of two PA66 batches.
Sample masses: 11.96 mg (blue) and 11.85 mg (red);
heating to 330°C at 20 K/min after cooling at 20 K/min, dynamic N2
atmosphere.
Oxidative Stability
OIT tests (oxidative-induction time) are well-known for evalu-
ating the resistance to oxygen of polymers, in particular
polyolefins. In this example, two PP samples were heated to 200°C
under a dynamic nitrogen atmosphere. The endothermic peaks detected
during heating illustrate the melting of the polypropylene. After 3
minutes at 200°C, the gas was switched to air. The resulting
exothermic effects indicate the polymer degradation. In the present
case, oxidation occurs earlier for sample A than for sample B (OIT
6.6 min vs. 11.6 min). OIT test on PP. Sample masses: 9.48 mg
(sample A) and 9.55 mg (sample B);
heating to 200°C at 20 K/min under N2 (50 ml/min), 3 min isothermal
under N2, isothermal under air (50 ml/min) until degradation.
Applications
13
exo
120
140
160
180
200
220
240
260
280
300
Time/min
Isothermal Crystallization of a Semi-Crystalline
Thermoplastic
Isothermal crystallization tests are often used to simulate the
rapid cooling of polymer parts during production (e.g., injection
molding). The graph on the left depicts an isothermal crystalliza-
tion experiment on PA66 GF30 (containing 30 wt% glass fiber) using
the DSC 214 Polyma in combination with the IC70 intra- cooler. The
low thermal mass of the Arena® furnace allows for a temperature
interval of almost 60 K to be bridged within seconds. Based on
this, it is possible to separate solidification of PA66 from the
starting phase of the isothermal segment. This clearly demonstrates
the superior cooling performance of the heat-flux DSC 214
Polyma.
Isothermal crystallization of a semi-crystalline thermoplastic.
11.4 mg PA66 GF30 in a dynamic nitrogen atmosphere, intracooler for
the temperature range -70°C to 600°C. The temperature curve is
marked in red; the DSC curve in blue. The total crystallization
enthalpy at 237°C amounts to approx. 30 J/g. Important for
isothermal crystallization experiments is to avoid any
temperature-undershoot while changing over from cooling to the
isothermal phase.
14
Material A Material B
106.8 °C 97.0 °C
125.9 °C 123.5 °C
Temperature/°C
Material A Material B
Failure Analysis − Influence of Recycled Material
In this example, two recycled polypropylenes were being used for
injection molding. Material A was completely crystallized after the
molding process whereas material B was still molten. To discover
the reason for the differing behavior, DSC measurements were
performed.
Different solidification of two recycled PP samples. Sample mass:
approx. 13 mg; cooling at 10 K/min after heating to 200°C; dynamic
N2 atmosphere.
Melting of recycled PP with different PE contamination. Sample
mass: approx. 13 mg; heating to 200°C at 10 K/min after cooling at
10 K/min; dynamic N2 atmosphere.
The exothermic peaks appearing during cooling can be attributed to
crystallization of the polymer. Recycled material A starts to
crystallize at a higher temperature (endset temperature at 126°C,
blue curve) than the second material (endset temperature at only
122°C, red curve). Furthermore, in addition to the peaks at 121°C
(blue curve) and 118°C (red curve), a peak at 97°C (blue curve) and
a shoulder at 107°C (red curve) occur – clear indications for the
presence of a second component. The additional components in
material A cause earlier nucleation.
An Essential Aid for Process Optimization
The 2nd heating reveals further information. Besides the peaks at
165°C and 163°C, which are typical for the melting of polypro-
pylene, the blue curve exhibits two additional peaks at 110°C and
124°C, indicating the existence of additional LDPE, LLDPE or HDPE.
In contrast with this, material B has only one further peak at
126°C.
Temperature/°C
2nd heating 1st heating
Glass Transition: Mid: -47.2 °C Delta Cp*: 0.455 J/(gK)
Glass Transition: Mid: -47.1 °C Delta Cp*: 0.445 J/(gK)
Partial Area: 4.88 J/g 1.9 °C ... 32.5 °C 36.71 %
Area: -6.44 J/g Peak: 168.7 °C
Area: 4.85 J/g Peak: 32.7 °C 58.4 °C
18.0 °C
Low-Temperature Performance of Rubber
DSC measurements are important for rubbers used in tires because
their service temperature range is limited by the glass transition
temperature. In this example, an SBR sample was measured twice
between -100°C and 220°C. The endothermic step detected at -47°C
(mid-point) in both heating sequences is associated with the glass
transition of SBR. Between 0°C and 70°C, endothermic effects are
detected. They are most probably caused by the melting of
additives. The exothermic peak at 169°C (peak temperature),
exhibited only in the 1st heating, is due to post-vulcanization of
the elastomer.
Thermal behavior of SBR rubber. Sample mass: 15.41 mg; heating from
-100°C to 220°C at 10 K/min, twice; dynamic N2 atmosphere.
16
0.14
0.16
0.18
0.20
0.22
0.24
0.26
0.28
0.30
0.32
↓ exo 1st heating 2nd heating
As an amorphous polymer, this epoxy resin exhibits a glass
transition at 77°C (midpoint) with a specific heat capacity of 0.14
J/(g·K) in the 1st heating (blue) followed by an exothermal effect
(peak temperature 174°C), due to post-curing of the resin. As a
result of the post-curing, the glass transition temperature in the
2nd heating (green) is shifted to 88°C (midpoint). The step height
remains nearly the same. Since no further exothermal effect occurs,
it can be assumed that the epoxy resin was entirely cured during
the 1st heating.
Both the exothermal effect and the position (and shift) of the
glass transition temperature to higher values can be interpreted as
an evidence for the degree of curing of the material.
Sophisticated Measurement and Analysis
Epoxy Resin (EP)
Epoxy resins (EP) undergo a polyaddition cross-linking reaction.
The properties of the resin are strongly dependent on the
structure, the degree of cross linking, type and amount of the
reinforcement material and the processing procedure.
THERMOSETS
17
Indium Response Ratio > 100 mW/K**
Resolution (technical) 0.1 µW
Enthalpy precision · ± 0.1% for indium · ± 0.05% to ± 0.2% for most
samples
Specific heat determination Optional
Temperature modulation Optional
Cooling device options · Compressed air cooling (RT to 600°C) ·
IC40 (-40°C to 600°C) · IC70 (-70°C to 600°C) · LN2, automatically
controlled (-170°C to 600°C)
Gas atmospheres Inert, oxidizing, static and dynamic
operation
Gas controller · Switches for 3 gases included · MFC for 3 gases,
optional
ASC Up to 20 samples and references, optional
Software Proteus®, including SmartMode, ExpertMode,
AutoCalibration, AutoCooling, AutoEvaluation, Identify, OIT,
predefined methods, etc. The software runs under the operating
systems, Windows® 7, Windows® 8.1. and Windows® 10
Technical Specifications
* Maximum rates depend upon the temperature ** Related to indium as
standard material under measurement conditions typically used for
polymer investigation (10 mg sample mass, 10 K/min heating rate,
nitrogen atmosphere)
18
19
LABORATORY
Training
Expertise in Service Our Expertise – Service
All over the world, the name NETZSCH stands for comprehensive
support and reliable service, before and after sale. Our qualified
personnel from the technical service and application departments
are always available for consultation.
In special training programs tailored for you and your employees,
you will learn to tap the full potential of your instrument.
To maintain and protect your investment, you will be accompanied by
our experienced service team over the entire life span of your
instrument.
The NETZSCH Thermal Analysis applications laborato- ries are a
proficient partner for nearly any Thermal Anal- ysis issue. Our
involvement in your projects begins with proper sample preparation
and continues through meticulous examination and interpretation of
the measurement results. Our diverse methods and over 30 different
state-of-the-art measuring stations will provide ready-made
solutions for all your thermal needs.
Within the realm of thermal analysis and the measure- ment of
thermo-physical properties, we offer you a comprehensive line of
the most diverse analysis tech- niques for materials
characterization.
Measurements can be carried out on samples of the most varied of
geometries and configurations. You will receive high-precision
measurement results and valu- able interpretations from us in the
shortest possible time. This will enable you to precisely
characterize new materials and components before actual deployment,
minimize risks of failure, and gain decisive advantages over your
competitors.
Our Expertise – Applications Laboratories
NETZSCH-Gerätebau GmbH Wittelsbacherstraße 42 95100 Selb Germany
Tel.: +49 9287 881-0 Fax: +49 9287 881 505 at@netzsch.com N
G B
· D SC
2 14
P ol
ym a
· E N
e.
The NETZSCH Group is an owner-managed, international technology
company with headquarters in Germany. The Business Units Analyzing
& Testing, Grinding & Dispersing and Pumps & Systems
represent customized solutions at the highest level. More than
3,700 employees in 36 countries and a worldwide sales and service
network ensure customer proximity and competent service. Our
performance standards are high. We promise our customers Proven
Excellence – exceptional performance in everything we do, proven
time and again since 1873.