Post on 29-Nov-2019
transcript
EDMS NO. REV. VALIDITY
1512110 0.0 APPROVED
REFERENCE
J3022578
Date: 2015-05-08
CERN CH1211 Geneva 23 Switzerland
ELECTRON BEAM WELDING
PROCEDURE QUALIFICATION RECORD
WPQR (QMOB)
N° EBW‐2015‐01
CCC CRYOSTAT
DOCUMENT PREPARED BY: DOCUMENT CHECKED BY: DOCUMENT APPROVED BY:
Paula Freijedo Menendez Thierry Tardy EN/MME-FW
J. Pierre Brachet
EN-MME-FW
Gilles Favre EN-MME-FW
BPQR N° / REFERENCE EDMS NO. REV. VALIDITY
B-2015-01 / J3022578 1512110 0.0 APPROVED
Page 2
TABLE OF CONTENTS
GENERAL INFORMATION .............................................................................................................. 3
RECORD EBW TEST ....................................................................................................................... 3
RESULT TESTS ............................................................................................................................... 6
ANNEX (ES) ................................................................................................................................... 6
BPQR N° / REFERENCE EDMS NO. REV. VALIDITY
B-2015-01 / J3022578 1512110 0.0 APPROVED
Page 3
2‐ RECORD EBW TEST
Equipment Type PTR
Join type BW
Depth of penetration Q‐1: 1mm / Q‐1.5:1.5mm
Filler metal N.A
Vacuum 5 x 10-4
Welding position PA
Other information: See p‐WPS 2015‐026‐FW & 2015‐027‐FW for welding parameters (See Annex 1)
ASSEMBLY DESIGN
Q‐1: Thickness 1mm
Q‐1.5: Thickness 1.5mm
1‐ GENERAL INFORMATION
REFERENCE P‐WPS: 2015‐026‐FW & 2015‐027‐FW
WELDING PROCESS:
ELECTRON BEAM WELDING
(N° 511 according to ISO 4063)
STANDARD REFERENCE:
ISO 15614‐11. Specification and qualification of
welding procedures for metallic materials‐ Welding
procedure Test‐ Electron and laser beam welding
WELD DATE: 24 / 02 / 2015
WELDER NAME: Thierry Tardy ID: ‐‐
N° SAMPLES: 2 ID. SAMPLES: Q‐1 & Q‐1.5
MANUFACTURER: CERN‐EN/MME‐FW NOTIFIED BODY : CERN INTERNAL QUALIFICATION
BASE METALS:
SPECIFICATION
/ GRADE STANDARD or REFERENCE
GROUP
ISO/TR
THICKNESS
(mm)
DIAMETER
(mm)
CERTIFICATE
EN 10204 3.1
1. 1.4429 / 316LN CERN THECNICAL
SPECIFICATION Nº1002 8.1 1 / 1 ‐ N°1 (Annex 2)
2. 1.4429 / 316LN CERN THECNICAL
SPECIFICATION Nº1002 8.1 1.5 / 1.5 ‐ N°2 (Annex 2)
BPQR N° / REFERENCE EDMS NO. REV. VALIDITY
B-2015-01 / J3022578 1512110 0.0 APPROVED
Page 4
HEAT TREATMENT: N.A
PROCEDURE
PREHEAT
TEMP
°C PREHEAT
TIME
POST HEAT
TEMP
POST HEAT
TIME
PWHT MIN °C PWHT
MAX
°C HEATING
RATE
°C/h COOLING RATE °C/h
CLEANING :
CLEANING METHOD BEFORE
WELDING Degreasing
CLEANING METHOD AFTER
WELDING ‐
PICTURES
WE CERTIFY THAT THE STATEMENT IN THIS RECORD ARE CORRECT AND THAT THE TESTS WELDS PREPARED, WELDED AND TESTED SATISFACTORILY IN ACCORDANCE WITH THE
REQUERIMENTS OF ISO‐15614‐11 INDICATED ABOVE
BPQR N° / REFERENCE EDMS NO. REV. VALIDITY
B-2015-01 / J3022578 1512110 0.0 APPROVED
Page 5
3‐ RESULTS TEST
SEQUENCE TEST STANDARD ACCEPTANCE
CRITERIA RESULTS REPORT N°
VISUAL INSPECTION ISO 17637 EN ISO 13919‐1
Level B SATISFACTORY ‐
DYE PENETRANT ISO 3452‐1 EN ISO 13919‐1
Level B SATISFACTORY ‐
RADIOGRAPHIC
EXAMINATION EN 17636‐2
EN ISO 13919‐1
Level B SATISFACTORY
EDMS Nº1507381
https://edms.cern.ch/document/1507381/1
TENSILE TEST
Tensile strength of the
specimen shall not be lower
than the minimum value
specified for the application
indicated in CERN THECNICAL
SPECIFICATION Nº1002 Ed.5
SATISFACTORY EDMS Nº 1502555
https://edms.cern.ch/document/1502555/1
METALLOGRAPHIC
EXAMINATION EN 17639
EN ISO 13919‐1
Level B SATISFACTORY
Q‐1 : EDMS N°1502555 &
https://edms5.cern.ch/document/1502555/1
Q ‐1.5 : EDMS Nº1505509
https://edms5.cern.ch/document/1505509/1
BPQR N° / REFERENCE EDMS NO. REV. VALIDITY
B-2015-01 / J3022578 1512110 0.0 APPROVED
Page 6
4‐ ANNEX (ES) :
ANNEX N°1: P‐WPS
ANNEX N°2: MATERIAL CERTIFICATES
‐ N‐1: STAINLESS‐STEEL CERTIFICATE THICKNESS 1MM
‐ N‐2: STAINLESS‐STEEL CERTIFICATE THICKNESS 1.5MM
Page 1 of 2
CERN CH‐1211 Geneva 23 Switzerland
EUROPEAN ORGANIZATION FOR NUCLEAR RESEARCH
1211 Geneva 23 ‐ Switzerland
WELDING PROCEDURE SPECIFICATION – EBW
Preliminary
WPS No.: 2015‐026‐FW Rev.: 0 Date: 25‐02‐2015
Operator: T. Tardy Machine: PTR Location: Building 100
Ref. WPQR: Ref. standard: ISO 15614‐11 Job No.: J3022578
Client: Lees Andrew John Project: CCC Cryostat
PREPARATION
Joint configuration: Butt weld Joint type: N.A. Single/Double: Single side
Cleaning: Welding position: PA Backing: Yes
JOINT SKETCH
PARENT METAL(S) Name / Grade Standard Group Delivery cond. Thickness (mm) Diameter(mm)
I 316LN / 1.4429 EN 10028‐7 8.1 1 ‐ II 316LN / 1.4429 EN 10028‐7 8.1 1 ‐
FILLER METAL
Trade name Classification Group
I N.A.
II
WELDING PARAMETERS
Working distance (mm): 400 HV (KV): SW: N.A. Vacuum (mbar): 5 x 10‐4
First pass Second pass Third pass
Foc (mA) 1000 / 420
Ibeam(mA) 7,5
Welding speed(mm/s) 16,7
Slope in (mm/°) 5mm
Overlap (mm/°) 10°
Slope out (mm/°) 5mm
Deflection
Pattern No. 1
Frequency (Hz) 100
Amplitude X 15
Amplitude Y 0
Pulsation
Frequency (Hz): N.A
Duty (%): N.A
Mode: N.A
Pulse (mA): N.A
Ratio: N.A
Page 2 of 2
CERN CH‐1211 Geneva 23 Switzerland
TACKING PARAMETERS
Foc (mA): 1000 / 420 Ibeam(mA): 7,5 Welding speed(mm/s): 16,7
Slope in (mm/°): 5mm Length (mm/°): Slope out (mm/°): 5
Deflection pattern No.: 1 Freq. (Hz): Amplitude(mm) X: 15 Y:0
Pulsation freq. (Hz): N.A. Duty (%):N.A. Mode: N.A Pulse(mA): N.A Ratio: N.A
BEAM CALIBRATION
IH (%):N.A. ALIG X: N.A. ALIG Y: N.A.
UBIAS (V): N.A. STIG X: N.A. STIG Y: N.A.
HEAT TREATMENT
Preheat temp.(°C): N.A. Interpass temp.(°C): N.A. PWHT procedure: N.A.
ADDITIONAL COMMENTS
ADDITIONAL INFO ENCLOSED
Approved by
Thierry Tardy
Date
17/03/15
Signature
Page 1 of 2
CERN CH‐1211 Geneva 23 Switzerland
EUROPEAN ORGANIZATION FOR NUCLEAR RESEARCH
1211 Geneva 23 ‐ Switzerland
WELDING PROCEDURE SPECIFICATION – EBW
Preliminary
WPS No.: 2015‐027‐FW Rev.: 0 Date: 25‐02‐2015
Operator: T. Tardy Machine: PTR Location: Building 100
Ref. WPQR: Ref. standard: ISO 15614‐11 Job No.: J3022578
Client: Lees Andrew John Project: CCC Cryostat
PREPARATION
Joint configuration: Butt weld Joint type: N.A. Single/Double: Single side
Cleaning: Welding position: PA Backing: Yes
JOINT SKETCH
PARENT METAL(S) Name / Grade Standard Group Delivery cond. Thickness (mm) Diameter(mm)
I 316LN / 1.4429 EN 10028‐7 8.1 1.5 ‐ II 316LN / 1.4429 EN 10028‐7 8.1 1.5 ‐
FILLER METAL
Trade name Classification Group
I N.A.
II
WELDING PARAMETERS
Working distance (mm): 400 HV (KV): SW: N.A. Vacuum (mbar): 5 x 10‐4
First pass Second pass Third pass
Foc (mA) 1000 / 420
Ibeam(mA) 9,5
Welding speed(mm/s) 16,7
Slope in (mm/°) 5mm
Overlap (mm/°) 10°
Slope out (mm/°) 5mm
Deflection
Pattern No. 1
Frequency (Hz) 100
Amplitude X 15
Amplitude Y 0
Pulsation
Frequency (Hz): N.A
Duty (%): N.A
Mode: N.A
Pulse (mA): N.A
Ratio: N.A
Page 2 of 2
CERN CH‐1211 Geneva 23 Switzerland
TACKING PARAMETERS
Foc (mA): 1000 / 420 Ibeam(mA): 5 Welding speed(mm/s): 16,7
Slope in (mm/°): 5mm Length (mm/°): Slope out (mm/°): 5mm
Deflection pattern No.: 1 Freq. (Hz): 100 Amplitude(mm) X: 15 Y: 0
Pulsation freq. (Hz): N.A. Duty (%):N.A. Mode: N.A Pulse(mA): N.A Ratio: N.A
BEAM CALIBRATION
IH (%):N.A. ALIG X: N.A. ALIG Y: N.A.
UBIAS (V): N.A. STIG X: N.A. STIG Y: N.A.
HEAT TREATMENT
Preheat temp.(°C): N.A. Interpass temp.(°C): N.A. PWHT procedure: N.A.
ADDITIONAL COMMENTS
ADDITIONAL INFO ENCLOSED
Approved by
Thierry Tardy
Date
17/03/15
Signature