Post on 05-Apr-2018
transcript
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 1/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 2/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 3/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 4/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 5/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 6/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 7/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 8/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 9/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 10/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 11/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 12/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 13/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 14/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 15/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 16/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 17/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 18/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 19/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 20/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 21/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 22/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 23/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 24/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 25/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 26/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 27/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 28/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 29/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 30/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 31/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 32/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 33/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 34/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 35/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 36/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 37/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 38/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 39/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 40/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 41/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 42/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 43/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 44/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 45/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 46/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 47/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 48/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 49/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 50/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 51/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 52/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 53/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 54/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 55/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 56/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 57/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 58/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 59/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 60/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 61/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 62/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 63/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 64/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 65/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 66/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 67/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 68/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 69/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 70/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 71/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 72/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 73/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 74/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 75/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 76/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 77/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 78/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 79/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 80/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 81/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 82/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 83/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 84/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 85/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 86/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 87/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 88/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 89/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 90/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 91/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 92/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 93/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 94/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 95/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 96/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 97/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 98/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 99/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 100/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 101/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 102/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 103/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 104/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 105/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 106/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 107/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 108/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 109/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 110/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 111/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 112/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 113/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 114/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 115/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 116/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 117/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 118/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 119/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 120/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 121/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 122/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 123/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 124/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 125/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 126/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 127/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 128/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 129/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 130/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 131/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 132/257
WWW.WELD.4T.COM
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 133/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 134/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 135/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 136/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 137/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 138/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 139/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 140/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 141/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 142/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 143/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 144/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 145/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 146/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 147/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 148/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 149/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 150/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 151/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 152/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 153/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 154/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 155/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 156/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 157/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 158/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 159/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 160/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 161/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 162/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 163/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 164/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 165/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 166/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 167/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 168/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 169/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 170/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 171/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 172/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 173/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 174/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 175/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 176/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 177/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 178/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 179/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 180/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 181/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 182/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 183/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 184/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 185/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 186/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 187/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 188/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 189/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 190/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 191/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 192/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 193/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 194/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 195/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 196/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 197/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 198/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 199/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 200/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 201/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 202/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 203/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 204/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 205/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 206/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 207/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 208/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 209/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 210/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 211/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 212/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 213/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 214/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 215/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 216/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 217/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 218/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 219/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 220/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 221/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 222/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 223/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 224/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 225/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 226/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 227/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 228/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 229/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 230/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 231/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 232/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 233/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 234/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 235/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 236/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 237/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 238/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 239/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 240/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 241/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 242/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 243/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 244/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 245/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 246/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 247/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 248/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 249/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 250/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 251/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 252/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 253/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 254/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 255/257
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 256/257
WWW.WELD.4T.COM
7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul
http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 257/257