M.S.Trn Ngc Dân 19 Sep 02 Copy from Welding Inspection Defects/Repairs Course Reference WIS 5
Transcript
Page 1: Copy from Welding Inspectionkruwelding.com/expert/WIS5 DEFECT.pdf · Copy from Welding Inspection Defects/Repairs Course Reference WIS 5. M.S.Trần Ngọc Dân ... A welding inspector

M.S.Trần Ngọc Dân

19 Sep 02

Copy from

Welding InspectionDefects/Repairs

Course Reference WIS 5

Page 2: Copy from Welding Inspectionkruwelding.com/expert/WIS5 DEFECT.pdf · Copy from Welding Inspection Defects/Repairs Course Reference WIS 5. M.S.Trần Ngọc Dân ... A welding inspector

M.S.Trần Ngọc Dân

19 Sep 02

Weld DefectsDefects which may be detected by visual

inspection can be grouped under five headings

Cracks

Surface irregularities

Contour defects

Root defects

Miscellaneous

Page 3: Copy from Welding Inspectionkruwelding.com/expert/WIS5 DEFECT.pdf · Copy from Welding Inspection Defects/Repairs Course Reference WIS 5. M.S.Trần Ngọc Dân ... A welding inspector

M.S.Trần Ngọc Dân

19 Sep 02

Weld Defects

Other associated defects

Cavities

Solid inclusions

Set up irregularities

Parent material defects

Page 4: Copy from Welding Inspectionkruwelding.com/expert/WIS5 DEFECT.pdf · Copy from Welding Inspection Defects/Repairs Course Reference WIS 5. M.S.Trần Ngọc Dân ... A welding inspector

M.S.Trần Ngọc Dân

19 Sep 02

Cracks

Hydrogen (HICC)

Solidification (Hot tears)

Reheat cracks

Lamellar tearing

The four essential crack mechanisms

Page 5: Copy from Welding Inspectionkruwelding.com/expert/WIS5 DEFECT.pdf · Copy from Welding Inspection Defects/Repairs Course Reference WIS 5. M.S.Trần Ngọc Dân ... A welding inspector

M.S.Trần Ngọc Dân

19 Sep 02

Cracks

Longitudinal parent metal crack Transverse weld metal crack

Longitudinal weld metal crack Lamellar tearing

Page 6: Copy from Welding Inspectionkruwelding.com/expert/WIS5 DEFECT.pdf · Copy from Welding Inspection Defects/Repairs Course Reference WIS 5. M.S.Trần Ngọc Dân ... A welding inspector

M.S.Trần Ngọc Dân

19 Sep 02 Transverse crack Center line crack

Page 7: Copy from Welding Inspectionkruwelding.com/expert/WIS5 DEFECT.pdf · Copy from Welding Inspection Defects/Repairs Course Reference WIS 5. M.S.Trần Ngọc Dân ... A welding inspector

M.S.Trần Ngọc Dân

19 Sep 02

Surface Irregularities

Page 8: Copy from Welding Inspectionkruwelding.com/expert/WIS5 DEFECT.pdf · Copy from Welding Inspection Defects/Repairs Course Reference WIS 5. M.S.Trần Ngọc Dân ... A welding inspector

M.S.Trần Ngọc Dân

19 Sep 02

UndercutAn irregular groove at the toe of a weld run in

the parent metal

Excessive amps/volts

Excessive travel speed

Incorrect electrode angle

Excessive weaving

Incorrect welding technique

Electrode too large

Page 9: Copy from Welding Inspectionkruwelding.com/expert/WIS5 DEFECT.pdf · Copy from Welding Inspection Defects/Repairs Course Reference WIS 5. M.S.Trần Ngọc Dân ... A welding inspector

M.S.Trần Ngọc Dân

19 Sep 02

Cap Undercut

Page 10: Copy from Welding Inspectionkruwelding.com/expert/WIS5 DEFECT.pdf · Copy from Welding Inspection Defects/Repairs Course Reference WIS 5. M.S.Trần Ngọc Dân ... A welding inspector

M.S.Trần Ngọc Dân

19 Sep 02 Cap undercutRoot undercut

Page 11: Copy from Welding Inspectionkruwelding.com/expert/WIS5 DEFECT.pdf · Copy from Welding Inspection Defects/Repairs Course Reference WIS 5. M.S.Trần Ngọc Dân ... A welding inspector

M.S.Trần Ngọc Dân

19 Sep 02

OverlapAn imperfection at the toe or root of a weld caused by

metal flowing on to the surface of the parent metal

without fusing to it

Contamination

Slow travel speed

Incorrect welding

technique

Current too low

Page 12: Copy from Welding Inspectionkruwelding.com/expert/WIS5 DEFECT.pdf · Copy from Welding Inspection Defects/Repairs Course Reference WIS 5. M.S.Trần Ngọc Dân ... A welding inspector

M.S.Trần Ngọc Dân

19 Sep 02

Overlap

Page 13: Copy from Welding Inspectionkruwelding.com/expert/WIS5 DEFECT.pdf · Copy from Welding Inspection Defects/Repairs Course Reference WIS 5. M.S.Trần Ngọc Dân ... A welding inspector

M.S.Trần Ngọc Dân

19 Sep 02

Crater Pipe

Crater pipe is a shrinkage defect and not a gas defect, it

has the appearance of a gas pore in the weld crater

Too fast a cooling rate

Deoxidization

reactions and liquid to

solid volume change

Contamination

Crater crack

(Star crack)

Page 14: Copy from Welding Inspectionkruwelding.com/expert/WIS5 DEFECT.pdf · Copy from Welding Inspection Defects/Repairs Course Reference WIS 5. M.S.Trần Ngọc Dân ... A welding inspector

M.S.Trần Ngọc Dân

19 Sep 02

Crater Pipe

Crater pipe

Weld crater

Page 15: Copy from Welding Inspectionkruwelding.com/expert/WIS5 DEFECT.pdf · Copy from Welding Inspection Defects/Repairs Course Reference WIS 5. M.S.Trần Ngọc Dân ... A welding inspector

M.S.Trần Ngọc Dân

19 Sep 02

Contour Defects

Page 16: Copy from Welding Inspectionkruwelding.com/expert/WIS5 DEFECT.pdf · Copy from Welding Inspection Defects/Repairs Course Reference WIS 5. M.S.Trần Ngọc Dân ... A welding inspector

M.S.Trần Ngọc Dân

19 Sep 02

Contour Defects

Incomplete filled groove Poor cap profile

Excessive cap heightIncomplete filled groove

+ Lack of sidewall fusion

Page 17: Copy from Welding Inspectionkruwelding.com/expert/WIS5 DEFECT.pdf · Copy from Welding Inspection Defects/Repairs Course Reference WIS 5. M.S.Trần Ngọc Dân ... A welding inspector

M.S.Trần Ngọc Dân

19 Sep 02Incomplete filled grooveExcess cap reinforcement

Page 18: Copy from Welding Inspectionkruwelding.com/expert/WIS5 DEFECT.pdf · Copy from Welding Inspection Defects/Repairs Course Reference WIS 5. M.S.Trần Ngọc Dân ... A welding inspector

M.S.Trần Ngọc Dân

19 Sep 02

Root Defects

Page 19: Copy from Welding Inspectionkruwelding.com/expert/WIS5 DEFECT.pdf · Copy from Welding Inspection Defects/Repairs Course Reference WIS 5. M.S.Trần Ngọc Dân ... A welding inspector

M.S.Trần Ngọc Dân

19 Sep 02

Root Defects

Incomplete root fusion

Incomplete root penetration

Low Amps/volts

Large Root face

Small Root Gap

Fast Travel Speed

Incorrect Electrode

Angle

Contamination

Page 20: Copy from Welding Inspectionkruwelding.com/expert/WIS5 DEFECT.pdf · Copy from Welding Inspection Defects/Repairs Course Reference WIS 5. M.S.Trần Ngọc Dân ... A welding inspector

M.S.Trần Ngọc Dân

19 Sep 02

Root Defects

Lack of root fusionLack of root Penetration

Page 21: Copy from Welding Inspectionkruwelding.com/expert/WIS5 DEFECT.pdf · Copy from Welding Inspection Defects/Repairs Course Reference WIS 5. M.S.Trần Ngọc Dân ... A welding inspector

M.S.Trần Ngọc Dân

19 Sep 02Lack of root fusionLack of root penetration

Page 22: Copy from Welding Inspectionkruwelding.com/expert/WIS5 DEFECT.pdf · Copy from Welding Inspection Defects/Repairs Course Reference WIS 5. M.S.Trần Ngọc Dân ... A welding inspector

M.S.Trần Ngọc Dân

19 Sep 02

Concave root

Root Defects

Root faces too large

Root gap too large

Excessive back purge

pressure during TIG welding

Excessive root bead grinding

before the application of the

second pass

A shallow groove, which may occur in the root of a butt weld

Page 23: Copy from Welding Inspectionkruwelding.com/expert/WIS5 DEFECT.pdf · Copy from Welding Inspection Defects/Repairs Course Reference WIS 5. M.S.Trần Ngọc Dân ... A welding inspector

M.S.Trần Ngọc Dân

19 Sep 02

Concave Root

Page 24: Copy from Welding Inspectionkruwelding.com/expert/WIS5 DEFECT.pdf · Copy from Welding Inspection Defects/Repairs Course Reference WIS 5. M.S.Trần Ngọc Dân ... A welding inspector

M.S.Trần Ngọc Dân

19 Sep 02

Excessive root penetration

Root Defects

Root faces too small

Root gap too large

Excessive amps/volts

Slow travel speed

Root penetration bead in excess in accordance with the

relevant specification being used

Page 25: Copy from Welding Inspectionkruwelding.com/expert/WIS5 DEFECT.pdf · Copy from Welding Inspection Defects/Repairs Course Reference WIS 5. M.S.Trần Ngọc Dân ... A welding inspector

M.S.Trần Ngọc Dân

19 Sep 02

Excessive Root Penetration

Page 26: Copy from Welding Inspectionkruwelding.com/expert/WIS5 DEFECT.pdf · Copy from Welding Inspection Defects/Repairs Course Reference WIS 5. M.S.Trần Ngọc Dân ... A welding inspector

M.S.Trần Ngọc Dân

19 Sep 02Concave root Excessive root penetration

Page 27: Copy from Welding Inspectionkruwelding.com/expert/WIS5 DEFECT.pdf · Copy from Welding Inspection Defects/Repairs Course Reference WIS 5. M.S.Trần Ngọc Dân ... A welding inspector

M.S.Trần Ngọc Dân

19 Sep 02

Shrinkage groove

Root Defects

Insufficient weld metal

deposited in the root

pass

Too fast a cooling rate

during the application of

the root bead pass

Poor welding technique

A shallow groove caused by contraction in the weld

metal along each side of the penetration bead

Page 28: Copy from Welding Inspectionkruwelding.com/expert/WIS5 DEFECT.pdf · Copy from Welding Inspection Defects/Repairs Course Reference WIS 5. M.S.Trần Ngọc Dân ... A welding inspector

M.S.Trần Ngọc Dân

19 Sep 02

Root Defects

Burn through

High Amps/volts

Small Root face

Large Root Gap

Slow Travel Speed

A localized collapse of the weld pool due to excessive

penetration resulting in a hole in the root run

Page 29: Copy from Welding Inspectionkruwelding.com/expert/WIS5 DEFECT.pdf · Copy from Welding Inspection Defects/Repairs Course Reference WIS 5. M.S.Trần Ngọc Dân ... A welding inspector

M.S.Trần Ngọc Dân

19 Sep 02 Burn through

Burn

Through

Page 30: Copy from Welding Inspectionkruwelding.com/expert/WIS5 DEFECT.pdf · Copy from Welding Inspection Defects/Repairs Course Reference WIS 5. M.S.Trần Ngọc Dân ... A welding inspector

M.S.Trần Ngọc Dân

19 Sep 02

Root Coking/Oxidized Root

Loss or insufficient

back purging gas

Most commonly

occurs when welding

stainless steels

Purging gases

include argon, helium

and occasionally

nitrogen

Page 31: Copy from Welding Inspectionkruwelding.com/expert/WIS5 DEFECT.pdf · Copy from Welding Inspection Defects/Repairs Course Reference WIS 5. M.S.Trần Ngọc Dân ... A welding inspector

M.S.Trần Ngọc Dân

19 Sep 02

Miscellaneous Defects

Page 32: Copy from Welding Inspectionkruwelding.com/expert/WIS5 DEFECT.pdf · Copy from Welding Inspection Defects/Repairs Course Reference WIS 5. M.S.Trần Ngọc Dân ... A welding inspector

M.S.Trần Ngọc Dân

19 Sep 02

Miscellaneous Defects

Arc strike

Accidental striking of

the arc onto the parent

material

Faulty electrode holder

Poor cable insulation

Poor return lead

clamping

Page 33: Copy from Welding Inspectionkruwelding.com/expert/WIS5 DEFECT.pdf · Copy from Welding Inspection Defects/Repairs Course Reference WIS 5. M.S.Trần Ngọc Dân ... A welding inspector

M.S.Trần Ngọc Dân

19 Sep 02

Spatter

Excessive current

Damp electrodes

Contamination

Incorrect wire feed

speed when welding

with the MAG welding

process

Miscellaneous Defects

Page 34: Copy from Welding Inspectionkruwelding.com/expert/WIS5 DEFECT.pdf · Copy from Welding Inspection Defects/Repairs Course Reference WIS 5. M.S.Trần Ngọc Dân ... A welding inspector

M.S.Trần Ngọc Dân

19 Sep 02

Inclusions

Page 35: Copy from Welding Inspectionkruwelding.com/expert/WIS5 DEFECT.pdf · Copy from Welding Inspection Defects/Repairs Course Reference WIS 5. M.S.Trần Ngọc Dân ... A welding inspector

M.S.Trần Ngọc Dân

19 Sep 02

Gas Cavities

Cluster porosityGas pore

Blow hole

Herringbone porosity

Root piping

Loss of gas shield

Damp electrodes

Contamination

Arc length too large

Damaged electrode flux

Moisture on parent material

Welding current to low

Page 36: Copy from Welding Inspectionkruwelding.com/expert/WIS5 DEFECT.pdf · Copy from Welding Inspection Defects/Repairs Course Reference WIS 5. M.S.Trần Ngọc Dân ... A welding inspector

M.S.Trần Ngọc Dân

19 Sep 02

Gas Cavities

Root piping

Porosity

Page 37: Copy from Welding Inspectionkruwelding.com/expert/WIS5 DEFECT.pdf · Copy from Welding Inspection Defects/Repairs Course Reference WIS 5. M.S.Trần Ngọc Dân ... A welding inspector

M.S.Trần Ngọc Dân

19 Sep 02 Single gas poreCluster porosity

Page 38: Copy from Welding Inspectionkruwelding.com/expert/WIS5 DEFECT.pdf · Copy from Welding Inspection Defects/Repairs Course Reference WIS 5. M.S.Trần Ngọc Dân ... A welding inspector

M.S.Trần Ngọc Dân

19 Sep 02

Solid Inclusions

Slag originates from welding

flux

MAG and TIG welding

process produce silica

inclusions

Slag is caused by

inadequate cleaning

Other inclusions include

tungsten and copper

inclusions from the TIG and

MAG welding process

Lack of sidewall fusion with

associated slag

Slag inclusions

Parallel slag lines

Slag inclusions are defined as a non-metallic inclusion

caused by some welding process

Page 39: Copy from Welding Inspectionkruwelding.com/expert/WIS5 DEFECT.pdf · Copy from Welding Inspection Defects/Repairs Course Reference WIS 5. M.S.Trần Ngọc Dân ... A welding inspector

M.S.Trần Ngọc Dân

19 Sep 02Elongated slag linesInterpass slag inclusions

Page 40: Copy from Welding Inspectionkruwelding.com/expert/WIS5 DEFECT.pdf · Copy from Welding Inspection Defects/Repairs Course Reference WIS 5. M.S.Trần Ngọc Dân ... A welding inspector

M.S.Trần Ngọc Dân

19 Sep 02

Set-up Irregularities

Plate/pipe Linear Misalignment

(Hi-Lo)

Poor fit-up

Angular Misalignment

Page 41: Copy from Welding Inspectionkruwelding.com/expert/WIS5 DEFECT.pdf · Copy from Welding Inspection Defects/Repairs Course Reference WIS 5. M.S.Trần Ngọc Dân ... A welding inspector

M.S.Trần Ngọc Dân

19 Sep 02

Linear Misalignment

Page 42: Copy from Welding Inspectionkruwelding.com/expert/WIS5 DEFECT.pdf · Copy from Welding Inspection Defects/Repairs Course Reference WIS 5. M.S.Trần Ngọc Dân ... A welding inspector

M.S.Trần Ngọc Dân

19 Sep 02

Parent Material Defects

A welding inspector should also inspect the parent

material for any visible defects

Lamination

Mechanical damage Lap

Segregation line

Page 43: Copy from Welding Inspectionkruwelding.com/expert/WIS5 DEFECT.pdf · Copy from Welding Inspection Defects/Repairs Course Reference WIS 5. M.S.Trần Ngọc Dân ... A welding inspector

M.S.Trần Ngọc Dân

19 Sep 02

Plate Lamination

Page 44: Copy from Welding Inspectionkruwelding.com/expert/WIS5 DEFECT.pdf · Copy from Welding Inspection Defects/Repairs Course Reference WIS 5. M.S.Trần Ngọc Dân ... A welding inspector

M.S.Trần Ngọc Dân

19 Sep 02

Weld Repairs

Page 45: Copy from Welding Inspectionkruwelding.com/expert/WIS5 DEFECT.pdf · Copy from Welding Inspection Defects/Repairs Course Reference WIS 5. M.S.Trần Ngọc Dân ... A welding inspector

M.S.Trần Ngọc Dân

19 Sep 02

A weld repair may be used to improve weld profiles

or extensive metal removal

Repairs to fabrication defects are generally easier

than repairs to service failures because the repair

procedure may be followed

The main problem with repairing a weld is the

maintenance of mechanical properties

During the inspection of the removed area prior to

welding the inspector must ensure that the defects

have been totally removed and the original joint

profile has been maintained as close as possible

Weld Repairs

Page 46: Copy from Welding Inspectionkruwelding.com/expert/WIS5 DEFECT.pdf · Copy from Welding Inspection Defects/Repairs Course Reference WIS 5. M.S.Trần Ngọc Dân ... A welding inspector

M.S.Trần Ngọc Dân

19 Sep 02

The specification or procedure will govern how the defective areas are to be removed. The

method of removal may be Grinding

Chipping

Machining

Filling

Arc air gouging

Oxy-gas gouging

Weld Repairs


Recommended