Deformation of polymer-metal laminates
Citation for published version (APA):Rastogi, R., Vellinga, W. P., & Meijer, H. E. H. (2001). Deformation of polymer-metal laminates. Poster sessionpresented at conference; Mate Poster Award 2001 : 6th Annual Poster Contest, .
Document status and date:Published: 01/01/2001
Document Version:Publisher’s PDF, also known as Version of Record (includes final page, issue and volume numbers)
Please check the document version of this publication:
• A submitted manuscript is the version of the article upon submission and before peer-review. There can beimportant differences between the submitted version and the official published version of record. Peopleinterested in the research are advised to contact the author for the final version of the publication, or visit theDOI to the publisher's website.• The final author version and the galley proof are versions of the publication after peer review.• The final published version features the final layout of the paper including the volume, issue and pagenumbers.Link to publication
General rightsCopyright and moral rights for the publications made accessible in the public portal are retained by the authors and/or other copyright ownersand it is a condition of accessing publications that users recognise and abide by the legal requirements associated with these rights.
• Users may download and print one copy of any publication from the public portal for the purpose of private study or research. • You may not further distribute the material or use it for any profit-making activity or commercial gain • You may freely distribute the URL identifying the publication in the public portal.
If the publication is distributed under the terms of Article 25fa of the Dutch Copyright Act, indicated by the “Taverne” license above, pleasefollow below link for the End User Agreement:
www.tue.nl/taverne
Take down policyIf you believe that this document breaches copyright please contact us at:
providing details and we will investigate your claim.
Download date: 22. Apr. 2019
� MNYJ[]VNW] XO VNLQJWRLJU NWPRWNN[RWP
��������������� ��������� � ������
2W YXUbVN[�VN]JU UJVRWJ]N\ ]QN VXM^UR JWM ]QN YUJ\]RL
MNOX[VJ]RXW KNQJ_RX^[ XO KX]Q VJ]N[RJU\ MN]N[VRWN ]QN
X_N[JUU KNQJ_RX^[ XO ]QN UJVRWJ]N ^YXW UXJMRWP� =QN
VNLQJWR\V Kb `QRLQ ]QN RW]N[OJLN MNOX[V\ R\ JW RW]N[YUJb
KN]`NNW ]QN RW]N[JL]RXW YX]NW]RJU JWM K^UT Y[XYN[]RN\ XO ]QN
RWMR_RM^JU VJ]N[RJU\�
;� ;J\]XPR� @�9� ?NUURWPJ� 1� .� 1� 6NRSN[.RWMQX_NW >WR_N[\R]b XO ]NLQWXUXPb� -NYJ[]VNW] XO 6NLQJWRLJU .WPRWNN[RWP
.aYN[RVNW]JU JYY[XJLQ+b JU]N[RWP ]QN K^UT Y[XYN[]RN\ XO JWb XWN XO ]QN ]`XVJ]N[RJU\ JWM XK\N[_RWP ]QN LQJWPN\ JWM RWOU^NWLN XW ]QNRW]N[OJLN `N LJW PN] J \]NY LUX\N[ RW ]X ^WMN[\]JWMRWP ]QN[XUN XO ]QN RW]N[OJLN M^[RWP UJVRWJ]N OX[VRWP� 1NWLN ]QNYXUbVN[ `J\ JWWNJUNM J] _J[RX^\ ]NVYN[J]^[N\ JWM ]QNLQJWPN\ XK\N[_NM XW
u ]QN VNLQJWRLJU KNQJ_RX^[ XO ]QN K^UT YXUbVN[�
u L[b\]JUURWR]b XO ]QN YXUbVN[�
u JMQN\RXW JWM MNOX[VJ]RXW VNLQJWR\V XO ]QN YXUbVN[ XW]QN UJVRWJ]N�
��
2W][XM^L]RXW
6N]QXM\ JWM 8K\N[_J]RXW\
0 0.5 1 1.5 2 2.5 30
20
40
60
80
100
120
λ2−λ−1 [−]
Tru
e st
ress
[MP
a]
PET, compression test
Pet Annealed from glass and Quenched
Amorphous 80°C 100°C Crystalline
170°C
120°C
135°C
210°C 260°C
0 0.5 1 1.5 2 2.5 30
20
40
60
80
100
120
λ2−λ−1 [−]
Tru
e st
ress
[MP
a]
PET, tensile test
Pet Annealed from glass and Quenched
amorp80° and 100°C
210°C
170°C 135°C
120°C crys
*#6NLQJWRLJU KNQJ_RX^[ XO K^UT YXUbVN[
9.= `J\ RWSNL]RXW VX^UMNM JWM JWWNJUNM J] _J[RX^\
]NVYN[J]^[N\ J\ \QX`W RW /RP�� OXUUX`NM Kb LXVY[N\\RXW
JWM ]NW\RUN UXJMRWP�
,# *MQN\RXW JWM MNOX[VJ]RXW XO YXUbVN[ XW ]QN UJVRWJ]N\
9.= LXJ]NM .UNL][XLQNVRLJUUb LXJ]NM \]NNU UJVRWJ]N\ `N[N
Y[NYJ[NM Kb KUXLT LXJ]RWP YXUbVN[ \XU^]RXW XW ]QN \]NNU
\^K\][J]N JWM L^]]RWP RW]X VRL[X ]NW\RUN KJ[\� 9.=�\]NNU
UJVRWJ]N\ `N[N JPJRW JWWNJUNM JWM Z^NWLQNM� =QN\N
JWWNJUNM UJVRWJ]N\ `N[N ]QNW UXJMNM RW ]NW\RXW ^\RWP ]QN
-NKNW 6RL[X�=NW\RUN ]N\]N[ JWM XK\N[_NM RW�\R]^ `R]Q ]QN
XY]RLJU VRL[X\LXYN ^WMN[ L[X\\ YXUJ[RcNM URPQ]�
/RP^[N �# <][JRWNM 9.=�\]NNU UJVRWJ]N\ XK\N[_NM ^WMN[ L[X\\�YXUJ[RcNM
URPQ] \QX` ]QN OX[VJ]RXW XO \QNJ[ KJWM\ JWM L[JLT\ RW ]QN YXUbVN[ OX[ J�
JVX[YQX^\ 9.= UJVRWJ]N� =QN UJVRWJ]N\ JWWNJUNM JKX_N K�����,� L�
����, JWM M� \UX`Ub L[b\]JUURcNM� MX WX] \QX` \QNJ[ KJWM\� K^] K[R]]UN
OJRU^[N JWM MNUJVRWJ]RXW�
+# ;NUJ]R_N L[b\]JUURWR]b XO ]QN YXUbVN[
=QN JWWNJUNM K^UT 9.= \JVYUN\ `N[N \]^MRNM ^\RWP /=
2WO[J�;NM \YNL][X\LXYb� =QN JK\X[Y]RXW KJWM J] ���"LV��
LJW KN ]JTNW J\ J [NON[NWLN ]X WX[VJURcN JUU \YNL][J ^\RWP
����LV�� JK\X[Y]RXW KJWM ]X MN]N[VRWN ]QN [NUJ]R_N
L[b\]JUURWR]b XO ]QN \JVYUN\�crystallinity vs. annealing temperature
0
0.2
0.4
0.6
0.8
1
1.2
0 50 100 150 200 250 300
annealing temp °C
crys
talli
nit
y ra
tio
,XWLU^\RXW\u 6NLQJWRLJU KNQJ_RX^[ XO 9.= LJW KN RWOU^NWLNM Kb
JWWNJURWP R] JKX_N R]\ LXUM L[b\]JUURcJ]RXW ]NVYN[J]^[N
�=LL&����,��
u *U]QX^PQ JWWNJURWP RVY[X_NM ]QN VNLQJWRLJU Y[XYN[]RN\
XO ]QN K^UT YXUbVN[� R] UNJM ]X `NJTNWRWP RW YXUbVN[�VN]JU
KXWMRWP�
u 1RPQN[ JWWNJURWP ]NVYN[J]^[N\ UNJM ]X YXX[N[ KXWMRWP�
u +XWMRWP UJbN[ MR[NL]Ub RW LXW]JL] `R]Q ]QN VN]JU \QX^UM KN
JVX[YQX^\ J\ L[b\]JUURWN LXJ]RWP MNUJVRWJ]N\ O[XV VN]JU
XW UXJMRWP�
/RP^[N �# 9N] `J\ JWWNJUNM J] _J[RX^\ ]NVYN[J]^[N\ KN]`NNW =PJWM =
V�
/RP^[N �# *WWNJURWP JKX_N =LL� 9.= P[JM^JUUb UXX\N\ \][JRW \XO]NWRWP
KNQJ_RX^[� `R]Q RWL[NJ\N RW \][JRW QJ[MNWRWP JWM S^VY RW bRNUM \][N\\�
/RP^[N �# 2WL[NJ\N RW ]QN [NUJ]R_N L[b\]JUURWR]b `R]Q RWL[NJ\RWP JWWNJURWP
]NVYN[J]^[N�
a)
c) d)
b)
;= *WWNJURWP ]RVN&��VRW
:^NWLQNM
� ��,
!��,
����,
� ��,����,����,
����,
2WSNL]RX
WVX^UMNM
=V&� ��,
=LL&����,
=P& ��,