230
Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis by Jason Philip Coyle A thesis submitted to the Faculty of Graduate and Postdoctoral Affairs in partial fulfillment of the requirements for the degree of Doctor of Philosophy in Chemistry Carleton University Ottawa, Ontario © 2014, Jason Philip Coyle
Transcript
Page 1: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

Group 11 Precursors for Atomic Layer Deposition: Design

and Synthesis of Advanced Precursors Enabled by

Investigations in Thermolysis

by

Jason Philip Coyle

A thesis submitted to the Faculty of Graduate and Postdoctoral

Affairs in partial fulfillment of the requirements for the degree of

Doctor of Philosophy

in

Chemistry

Carleton University

Ottawa, Ontario

© 2014, Jason Philip Coyle

Page 2: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

ii

Abstract

Atomic layer deposition (ALD) of copper seed layers for electrochemical

deposition of copper will likely be a step in fabricating future copper interconnects of

microelectronic devices. Development of precursors for copper ALD is necessary in

order to enable the deposition of suitable seed layers with acceptable properties.

Copper(I) amidinate compounds are leading precursor candidates for use in industry.

Modifications to their chemical structure was undertaken to improve precursor properties.

Copper(I) guanidinates were synthesized and used as single source precursors for copper

metal films at 225 °C. Their decomposition mechanism was investigated through solution

thermolysis experiments and by unravelling gas phase fragmentation pathways. Evidence

for CDI deinsertion occurring in solution was observed by NMR experiments while β-

hydrogen elimination was determined as the gas phase pathway by ToF-MS and MI-

FTIR experiments. Both pathways were rationalized by DFT calculations. Copper(I)

iminopyrrolidinate compounds were specifically designed to block CDI deinsertion and

β-hydrogen elimination. As a result, copper(I) tert-butyl-imino-2,2-dimethylpyrrolidinate

demonstrated superior thermal stability and adsorbed from the gas phase onto high

surface SiO2 at 275 °C with simultaneous loss of its tert-butyl group. Analogous silver(I)

and gold(I) compounds were demonstrated to be robust precursors for chemical vapour

deposition of metal films at deposition temperatures of 140 °C and 300 °C, respectively.

The lack of available monomeric copper(I) amidinate, guanidinate, and

iminopyrrolidinate compounds prompted synthetic work to employ N-heterocyclic

carbenes and acyclic diamino carbenes as Lewis bases in copper precursors. A large

series of monomeric copper(I) hexamethyldisilazide compounds were studied and

Page 3: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

iii

characterized extensively by thermal gravimetric analysis. Imidazolylidenes were

unsuitable for use in copper precursors due to thermal instability. Imidazolinylidenes and

formamidinylidenes fashioned several promising precursors demonstrating excellent

thermal stability and good volatility. The leading candidate, 1,3-diisopropyl-imidazolin-

2-ylidene copper hexamethyldisilazide, had a 1 Torr vapour pressure at 149 °C and could

be heated at 130 °C for two weeks without decomposition. Copper metal films were

deposited by plasma enhanced ALD at 225°C on SiO2.

Page 4: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

iv

Preface

This preface provides full bibliographical details for each article included in this

thesis, as well as whether the article is reproduced in whole or in part. Use of copyrighted

material is likewise acknowledged here. When citing material from this thesis, please cite

the article relevant to the chapter, if the chapter is based on a publication.

Pursuant to the Integrated Thesis policy of Carleton University, the supervisor

(Seán T. Barry) and the “student” (Jason P. Coyle) confirm that the student was fully

involved in setting up and conducting the research, obtaining data and analyzing results,

as well as preparing and writing the material presented in the co-authored articles(s)

integrated in the thesis. Additionally, the supervisor confirms the information provided

by the student in this preface.

Chapter 2

Coyle, J. P.; Monillas, W. H.; Yap. G. P. A.; Barry, S. T. “Synthesis and Thermal

Chemistry of Copper(I) Guanidinates” Inorg. Chem. 2008, 47, 683-689.

The article is wholly reproduced and edited for formatting and clarity of presentation.

Jason P. Coyle performed all work related to synthesis and characterization of

compounds, solution and gas phase thermolysis experiments, and deposition of copper

films. Crystallography was preformed by Wesley H. Monillas and Glenn P. A. Yap. The

article was written by Seán T. Barry.

Chapter 3

Coyle, J. P.; Johnson, P. A.; DiLabio, G. A.; Barry, S. T.; Müller, J. “Gas-Phase

Thermolysis of a Guanidinate Precursor of Copper Studied by Matrix Isolation, Time-of-

Flight Mass Spectrometry, and Computational Chemistry” Inorg. Chem. 2010, 49, 2844-

2850.

The article is wholly reproduced and edited for formatting and clarity of presentation.

The ΔG value for carbodiimide deinsertion in reference 16 was corrected to -44.4

kcal/mol along with an associated minor change to the body of text. Jason P. Coyle

performed all work related to synthesis and characterization of compounds, TOF MS and

MI FTIR experiments. Mechanistic DFT calculations were performed by Paul A. Johnson

supervised by Gino A. DiLabio. Jens Müller supervised the TOF MS and MI FTIR

experiments and calculated frequencies for trans-3. Writing was collaborative between

all co-authors.

Chapter 4

Coyle, J. P.; Kurek, A.; Pallister, P. J.; Sirianni, E. R.; Yap, G. P. A.; Barry, S. T.

“Preventing Thermolysis: Precursor Design for Volatile Copper Compounds” Chem.

Commun. 2012, 48, 10440-10442.

Page 5: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

v

Coyle, J. P.; Pallister, P. J.; Kurek, A.; Sirianni, E. R.; Yap, G. P. A.; Barry, S. T.

“Copper Iminopyrrolidinates: A Study of Thermal and Surface Chemistry” Inorg. Chem.

2013, 52, 910-917.

The articles are partially reproduced and edited to prevent repetition, formatting and

clarity of presentation. 1 Torr values for compounds 1–4 are different from the

publication because a calculation error was corrected. Partial results for the surface

studies are reproduced. Jason P. Coyle performed all work related to synthesis and

characterization of compounds, and thermo-gravimetric analysis. Solution thermolysis

experiments were performed by Agnes Kurek. Surface studies were performed by Peter J.

Pallister. Crystallography was performed by Eric R. Sirianni and Glenn P. A. Yap.

Writing was collaborative between all co-authors

Chapter 5

Coyle, J. P.; Gordon, P. G.; Wells. A. P.; Mandia, D. J.; Sirianni, E. R.; Yap, G. P. A.;

Barry, S. T. “Thermally Robust Gold and Silver Iminopyrrolidinates for Chemical Vapor

Deposition of Metal Films” Chem. Mater. 2013, 25, 4566-4573.

The article is wholly reproduced and edited for formatting and clarity of presentation.

Jason P. Coyle performed all work related to synthesis and characterization of

compounds, thermogravimetric analysis, gold film deposition and some film thickness

measurements by AFM. Peter G. Gordon performed depositions of the silver thin films,

thin film characterization by SEM and AFM, and resistivity measurments. Adam P.

Wells performed solution thermolysis experiments. David J. Mandia preformed XPS

characterizations. Crystallography was performed by Eric R. Sirianni and Glenn P. A.

Yap. Jason P. Coyle wrote the publication.

Chapter 6

Coyle, J. P.; Dey, G.; Sirianni, E. R.; Kemell, M. L.; Yap, G. P. A.; Ritala, M.; Leskelä,

M.; Elliott, S. D.; Barry, S. T. “Deposition of Copper by Plasma-Enhanced Atomic Layer

Deposition Using a Novel N-Heterocyclic Carbene Precursor” Chem. Mater. 2013, 25,

1132-1138.

The article is wholly reproduced and edited for formatting and clarity of presentation. 1

Torr values for compounds 1 and 2 are different from the publication because a

calculation error was corrected. Jason P. Coyle performed all work related to synthesis

and all characterizations of compounds including thermo-gravimetric analysis. PE-ALD

experiments of copper thin films were performed by Seán T. Barry, characterised by

Marianna L. Kemell, and supervised by Mikko Ritala and Markku Leskelä.

Crystallography was performed by Eric R. Sirianni and Glenn P. A. Yap. DFT calculated

surface models were performed by Gangotri Dey and supervised by Simon D. Elliott.

Writing was collaborative between all co-authors.

Page 6: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

vi

Chapter 7

Jason P. Coyle performed all work related to synthesis and characterization of

compounds including thermo-gravimetric analysis. Crystallography of compounds 2 and

7 were performed by Eric R. Sirianni and Glenn P. A. Yap. Crystallography of

compounds 8 and 10 were performed by Ilia Korobkov. Writing was collaborative

between Jason P. Coyle and Seán T. Barry.

Page 7: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

vii

Acknowledgements

I would like to thank Seán for inviting me to join his lab eight years ago. I started

as a volunteer and was immediately drawn to the excitement around making new

discoveries and the necessary high-level, social and technical discussions that would

follow. Unhesitatingly, I continued on as a co-op, honour, master, and doctoral student,

but these milestones were always secondary to just being a member of his lab. Every

discovery I made in the lab was met by an equal opportunity to explore its significance -

new equipment was purchased; conferences were attended; stints with collaborators were

funded; and partnerships in commercialization ventures were formed. Throughout my

time in the Barry Lab, Seán worked endlessly to improve or start facilities that his lab, the

chemistry department, and other faculties could share on top of being a popular and

effective teacher. Yet, working in his lab never seemed like work, nor was it expected to.

As I have realized from science, progress is easily limited by expectations. It has been a

great pleasure to be mentored by someone who expected nothing, but was prepared for

anything.

Although, I preferred to work solitarily in the lab, this was not considered “safe”,

so I would like to thank my fellow labmates over the years. Thank you Amanda, Allison,

Yamile, Pete, Julie, Todd, Paul, Agnes, Peter, Dave, Matt, Sara and the many others from

summer and honour projects for keeping me in awesome and “safe” company. Also,

thank you for your tolerance during my most serious and silliest of times.

I would like to express my gratitude towards the Chemistry Department’s

technical staff and their willingness to help or advise. Thank you Keith, Tony, Jim, Peter,

Susa, Tanya, Elena, Mastaneh, Graham, Daniel, and Shari for your kindness and support.

Page 8: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

viii

I would also like to thank Chantelle for keeping me on track near the tail end of my

studies.

Thank you to the members of the Ianoul Lab, the Manthorpe Lab, the DeRosa

Lab, and the Wang Lab for generously sharing your resources and knowledge whenever I

showed up at your doors.

On several occasions, I visited the lab of Dr. Jens Müller. His hospitality, support

and guidance concerning gas phase and synthetic techniques had a profound impact on

my development as a chemist. Of course, his students were largely responsible for the

fond memories. Thank you Nora, Bid, Nick, Sam, Saeid, Elaheh, and Subhayen for

welcoming and treating me as a full member of the lab. I would also like to thank Garth

and Darren for saving me from instrumentation failure and Cathy for help with arranging

my visits and orientation around the department.

Crystallographers were just a couple days away by FedEx in Delaware or a bus

ride to the University of Ottawa. Drs. Glenn Yap, Wesley Monillas, Eric Sirianni, and Ilia

Korobkov were always as keen to solve my samples as I was to send them. My syntheses

were never complete without a solved structure. Thank you.

Without disclosure, I have valued my interaction with GreenCentre Canada and

Parteq Innovations immensely. It was truly eye opening to work with their

commercialization and patent experts.

Lastly, I would like to thank Dave and Jeff at Applied Materials for my internship

experience and introduction to the ALD industry. Their lessons and knowledge were

invaluable to me, as a student, and sharpened my focus after I returned to Carleton. I am

Page 9: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

ix

also appreciative of the hospitality from Juhana, Wei-Min, and Satu during the brief time

I spent using reactors at Picosun.

Page 10: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

x

This thesis is dedicated to my parents, Anne Elizabeth and David George Coyle.

Page 11: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

xi

Table of Contents

Abstract .............................................................................................................................. ii

Preface ............................................................................................................................... iv

Acknowledgements ......................................................................................................... vii

Table of Contents ............................................................................................................. xi

List of Tables .................................................................................................................. xiv

List of Figures .................................................................................................................. xv

Abbreviations ................................................................................................................ xxii

Introduction ................................................................................................ 1 1 Chapter:

Motivation for Copper Seed Layers ............................................................................... 1 1.1

Atomic Layer Deposition ............................................................................................... 3 1.2

Copper Alkyl, Amido, and Alkoxide Complexes ........................................................... 4 1.3

Copper(I) Chloride ......................................................................................................... 7 1.4

Copper Precursors for Atomic Layer Deposition ........................................................... 8 1.5

1.5.1 Cu KI5 ........................................................................................................................ 9

1.5.2 Bis(tri-n-butylphosphine) Copper(I) acetylacetonate ............................................... 10

1.5.3 Copper(II) acetylacetonate precursors ..................................................................... 11

1.5.4 Copper(II) diketoiminate precursors ........................................................................ 13

1.5.5 Copper(I) and (II) dikitiminate precursors ............................................................... 14

1.5.6 Copper(I) amidinate precursors ................................................................................ 15

1.5.7 Copper(II) aminoalkoxide precursors ...................................................................... 16

1.5.8 Copper Precursor Summary ..................................................................................... 18

Upcoming Thesis Chapters ........................................................................................... 19 1.6

References .................................................................................................................... 20 1.7

Synthesis and Thermal Chemistry of Copper (I) Guanidinates ................. 27 2 Chapter:

Page 12: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

xii

Abstract ........................................................................................................................ 27 2.1

Introduction .................................................................................................................. 27 2.2

Results and Discussion ................................................................................................. 29 2.3

Conclusion .................................................................................................................... 43 2.4

Experimental................................................................................................................. 44 2.5

References .................................................................................................................... 46 2.6

Gas-Phase Thermolysis of a Guanidinate Precursor of Copper Studied by 3 Chapter:

Matrix Isolation, Time-of-Flight Mass Spectrometry and Computational Chemistry ..... 49

Abstract ........................................................................................................................ 49 3.1

Introduction .................................................................................................................. 51 3.2

Results and Discussion ................................................................................................. 52 3.3

Conclusion .................................................................................................................... 66 3.4

Experimental................................................................................................................. 67 3.5

Supplemental Information ............................................................................................ 71 3.6

References .................................................................................................................... 77 3.7

Copper Iminopyrrolidinates ....................................................................... 80 4 Chapter:

Abstract ........................................................................................................................ 80 4.1

Introduction .................................................................................................................. 81 4.2

Results and Discussion ................................................................................................. 84 4.3

Conclusion .................................................................................................................... 98 4.4

Experimental................................................................................................................. 99 4.5

References .................................................................................................................. 105 4.6

Thermally Robust Gold and Silver Iminopyrrolidinates for Chemical 5 Chapter:

Vapour Deposition of Metal Films ................................................................................. 108

Abstract ...................................................................................................................... 108 5.1

Introduction ................................................................................................................ 108 5.2

Page 13: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

xiii

Results and Discussion ............................................................................................... 112 5.3

Conclusion .................................................................................................................. 126 5.4

Experimental............................................................................................................... 127 5.5

Supplemental Information .......................................................................................... 132 5.6

References .................................................................................................................. 135 5.7

Deposition of Copper by Plasma-Enhanced Atomic Layer Deposition 6 Chapter:

Using a Novel N-Heterocyclic Carbene Precursor ......................................................... 139

Abstract ...................................................................................................................... 139 6.1

Introduction ................................................................................................................ 140 6.2

Results and Discussion ............................................................................................... 144 6.3

Conclusion .................................................................................................................. 153 6.4

Experimental............................................................................................................... 153 6.5

References .................................................................................................................. 157 6.6

Synthesis and Thermal Gravimetric Studies of Monomeric Cu(I)N(SiMe3)2 7 Chapter:

Complexes Supported by N-Heterocyclic and Acyclic Diamino Carbenes. .................. 162

Abstract ...................................................................................................................... 162 7.1

Introduction ................................................................................................................ 163 7.2

Results and Discussion ............................................................................................... 165 7.3

Conclusion .................................................................................................................. 179 7.4

Experimental Section .................................................................................................. 180 7.5

Supporting Information .............................................................................................. 188 7.6

References .................................................................................................................. 193 7.7

Conclusions .............................................................................................. 198 8 Chapter:

References .................................................................................................................. 205 8.2

Page 14: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

xiv

List of Tables

Table 2.1 Selected Crystal Data and Structure Refinement Parameters .......................... 32

Table 2.2 Selected bond lengths and angles for compounds 1 and 2. .............................. 33

Table 2.3 Thermal Decomposition Data for 1 - 3. ........................................................... 34

Table 4.1 Selected bond lengths and angles for 1 - 3. ...................................................... 87

Table 4.2 Kinetic data for the thermal decomposition of 1 – 4 at 165°C. The “correlation

coefficient” refers linear fit in Figure 4.9. ........................................................................ 95

Table 5.1 Crystal Data and Refinement Details of 1 and 2. ........................................... 114

Table 5.2 Selected Bond lengths and Angles for 1 and 2 .............................................. 115

Table 6.1 Selected bond lengths and bond angles for the structures of 1 and 2. ........... 146

Table 6.2 Computed Adsorption Energy ΔEad (kJ/mol) of the Precursors and Their

Probable by-Products on Two Surface Models - Cu55 with a Smooth (111) Surface and

Cu56 with One Extra Atom Making the Surface Rough.a ............................................... 152

Table 7.1 Properties of Diamino Carbene Cu(I) HMDS Compounds 1 – 10. ............... 167

Table 7.2 Selected Bond Lenghts and Bond Angles for the Structures of 2, 3, 5, 7, 8 and

10. aData was previously reported and provided for convenience.

8 ............................... 170

Table 7.3 Crystal Data and Structure Refinement Parameters. ...................................... 188

Page 15: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

xv

List of Figures

Figure 1.1 The copper ketoiminate precursor CuKI5 with a tethered vinyl-silyl Lewis

base. .................................................................................................................................... 9

Figure 1.2 Copper(II) acetylacetonate, R = H; tetramethylheptanedionate, R = Me;

hexafluoroacetylacetonate, R = F. .................................................................................... 12

Figure 1.3 Copper(II) 2-ethylimino-4-pentanonate ......................................................... 13

Figure 1.4 Asymmetric copper(I) and (II) dikitiminate precursors. ................................ 14

Figure 1.5 Copper(I)-N,Nʹ-di-sec-butylacetamidinate ..................................................... 15

Figure 1.6 Copper(II) aminoalkoxides, R = H, alkyl, fluoroalkyl. .................................. 17

Figure 2.1 Resonance Structures for Copper Amidinate and Guanidinate Ligands. ....... 28

Figure 2.2 Thermally Induced Carbodiimide Deinsertion. .............................................. 29

Figure 2.3 Single crystal X-ray structures for compounds 1 and 2. Hydrogen atoms were

omitted for clarity, and the thermal ellipses are shown at 30%. ....................................... 30

Figure 2.4 The dimer cores of (a) 1 and (b) 2, showing the twists induced by

pyramidalization of the chelating nitrogens. Except for the ligands’ sp2 carbon, all

carbon and hydrogen atoms are omitted for clarity, and the thermal ellipses are shown at

30%. .................................................................................................................................. 31

Figure 2.5 Thermogravimetric analyses of 1 (solid line), 2 (bold line), and 3 (grey line).

........................................................................................................................................... 34

Figure 2.6 Thermal Decomposition of Copper Guanidinates. ......................................... 36

Figure 2.7 Temperature-resolved mass spectrum of 1 showing the increase in

carbodiimide and a corresponding decrease in the dimethylamido diisopropyl guanidine.

........................................................................................................................................... 37

Figure 2.8 Temperature-resolved mass spectrum of 2 showing the increase in

carbodiimide and a corresponding decrease in the protonated triisopropyl guanidine

cation. ................................................................................................................................ 38

Figure 2.9 The temperature-resolved mass spectrum of 3 showing the increase in the

ligand fragment “C=NiPr” and a corresponding decrease in the protonated acetamidine

cation. ................................................................................................................................ 40

Page 16: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

xvi

Figure 2.10 Scanning electron micrograph of copper films deposited by (a) 1 and (b) 2.

........................................................................................................................................... 41

Figure 2.11 X-ray diffraction spectra of copper deposited in a CVD experiment using (a)

1 and (b) 2 as a precursor. ................................................................................................. 42

Figure 3.1 Decomposition of a Copper Guanidinate via CDI Deinsertion ...................... 51

Figure 3.2 Overview MS of the copper guanidinate 1 with thermolysis oven at 130 ºC

(no thermal fragmentation; bottom spectrum; M+ of 1 enlarged) and at 260 ºC (complete

thermal fragmentation of 1; top spectrum). ...................................................................... 53

Figure 3.3 Protonated and oxidized ligand with calculated masses. ................................ 54

Figure 3.4 Temperature dependence of intensities of selected ions arising from the

thermolysis of 1 [m/z = 466.3 (1+), 171.2 (2

+), 169.2 (3

+), 2.0 (H2

+) u]. .......................... 54

Figure 3.5 Decomposition of a Copper Guanidinate via β-hydride Elimination. ............ 55

Figure 3.6 Measured IR spectra of copper guanidinate 1 and its thermolysis products (x

axis, 1500 – 1800 cm-1

; y axis, absorbance). Spectrum A: 2 in solid argon (thermolysis

oven at 260 ºC); see Figure 3.13 for a complete IR spectrum. Spectrum B: results of a

thermolysis of complex 1 at 260 ºC; see Figure 3.12 for a complete IR spectrum.

Spectrum C: 3 in solid argon (thermolysis oven at 260 ºC); residual amounts of 2 have

been electronically eliminated; see Figure 3.14 for a complete IR spectrum. .................. 59

Figure 3.7 Possible isomers of 3 and the optimized structure for trans-3 obtained with

B3LYP/6-31+G(d,p)-DCP.. .............................................................................................. 61

Figure 3.8 Calculated fragmentation pathways for precursor 1. Free energies relative to

A1 for the reaction steps are shown (values in parentheses are relative to species 1) ...... 62

Figure 3.9 Temperature dependences of selected ions of the thermolysis at high

temperatures of 1 (spectrum B) and 2 (spectrum A) [m/z = 171.2 (2+), 169.2 (3

+), 126.2

(4+), 124.1 (CDI

+) 45.0 (HNMe2

+) u]. The intensities of masses at 169.2 and 124.1 u

were negligible in spectrum A (counts between 2 and 22 at sweep rates of 8 x 106). ...... 65

Figure 3.10 Carbodiimides. .............................................................................................. 65

Figure 3.11 Species 1 in solid argon (oven temperature at 140 ºC; no decomposition; 220

– 4000 cm-1

). Wavenumbers [cm-1

] of the marked IR bands are 2960.4, 2919.2, 2850.9,

2785.3, 1510.1, 1489.7, 1467.0, 1444.0, 1397.0, 1375.7, 1359.2, 1314.2, 1275.3, 1171.9,

1137.2, 1053.0, 783.2, 733.8, 457.4.................................................................................. 71

Figure 3.12 Results of a thermolysis of complex 1 at 260 ºC (220 – 4000 cm-1

; same IR

spectrum as Figure 3.6B). Wavenumbers [cm-1

] of the marked IR bands are 3012.8,

Page 17: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

xvii

2972.8, 2939.2, 2904.6, 2874.2, 2839.4, 2794.6, 1687.9, 1668.9, 1635.1, 1626.6, 1488.4,

1452.9, 1435.4, 1372.5, 1337.4, 1261.9, 1246.2, 1190.7, 1167.9, 1144.8, 1079.1, 1056.6,

1003.2, 942.5..................................................................................................................... 72

Figure 3.13 Species 2 in solid argon (thermolysis oven at 260 ºC; no decomposition; 220

– 4000 cm-1

; same IR spectrum as Figure 3.6A). The sample of 2 contained residual

amounts of iPrNCNiPr (CDI), which were electronically eliminated from the IR

spectrum of 2. Wavenumbers [cm-1

] of the marked IR bands are 3408.7, 3013.9, 2975.9,

2941.7, 2873.5, 2836.6, 2811.4, 2794.2, 1646.0, 1486.2, 1457.0, 1435.1, 1367.3, 1348.3,

1308.1, 1254.3, 1169.3, 1146.8, 1129.2, 1058.7, 1031.4, 937.3....................................... 73

Figure 3.14 Species 3 in solid argon (thermolysis oven at 260 ºC; no decomposition; 220

– 4000 cm-1

; same IR spectrum as Figure 3.6C). The sample of 2 contained small

amounts of iPrNCNiPr (CDI), which were electronically eliminated from the spectrum of

3. Wavenumbers [cm-1

] of the marked IR bands are 3012.9, 2973.4, 2939.3, 2874.6,

2839.5, 2794.5, 1687.9, 1668.9, 1634.9, 1626.7, 1488.5, 1452.2, 1436.8, 1372.3, 1337.3,

1261.9, 1246.1, 1190.7, 1167.6, 1144.6, 1079.4, 1003.2, 942.5....................................... 74

Figure 3.15 Results of a thermolysis of complex 2 at 700 ºC (220 – 4000 cm-1

).

Wavenumbers [cm-1

] of the marked IR bands are (assignments in parentheses) 3306.0,

2985.6 CDI), 2975.0 (HNMe2), 2940.6 (HNMe2), 2874.4 (HNMe2), 2832.3 (HNMe2),

2789.5 (HNMe2), 2123.5 (CDI; the structure of this IR band changes depending on the

way CDI is deposited in matrices; see reference L. C. Ziffle, A. P. Kenney, S. T. Barry

and J. Müller, Polyhedron, 2008, 27, 1832-1840.), 1645.9 (most intense peak of 2),

1457.6 (HNMe2), 1384.5 (CDI), 1368.4 (CDI), 1319.6 (CDI), 1306.7 (CDI), 1167.7

(CDI), 1150.4 (HNMe2), 1119.8 (CDI), 1020.9 (HNMe2), 935.8 (CDI), 908.6, 728.6

(most intense peak of HNMe2), 632.6 (CDI). The assignment of IR bands to HNMe2 is

based on an independently measured IR spectrum of matrix-isolated HNMe2 in argon (B.

Wittig, J. Müller, unpublished results).............................................................................. 75

Figure 3.16 Results of a thermolysis of complex 1 at 700 ºC (220 – 4000 cm-1

). Small

amounts of 2 and 3 were electronically eliminated from this spectrum. Wavenumbers

[cm-1

] of the marked IR bands are (assignments in parentheses) 2985.4, 2975.2 (HNMe2),

2940.7 (HNMe2), 2874.4 (HNMe2), 2832.3 (HNMe2), 2789.5 (HNMe2), 2127.7, 1649.2,

1483.3 (HNMe2), 1457.3 (HNMe2), 1439.1 (HNMe2), 1386.9, 1369.6, 1337.9, 1323.8,

1230.4, 1169.0, 1150.3 (HNMe2), 1106.0, 1021.0 (HNMe2), 929.1 (HNMe2), 866.6,

728.7 (most intense peak of HNMe2), 626.1. Note: The marked, but unassigned IR bands

could be tentatively assigned to the new carbodiimide 4. However, an unambiguous

characterization of 4 on the basis of the IR data alone is impossible. The IR band at

1649.2 cm-1

could be caused by the C=C stretching mode of 4 (see Figure 3.10). The

assignment of IR bands to HNMe2 is based on an independently measured IR spectrum of

matrix-isolated HNMe2 in argon (B. Wittig, J. Müller, unpublished results). .................. 76

Figure 4.1 Two Thermal Decomposition Pathways For a Copper(I) Guanidiante Species.

........................................................................................................................................... 82

Page 18: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

xviii

Figure 4.2 Series of Amidinate-Type Ligands with Differing Numbers of β-Hydrogens,

Shown As Their Corresponding Copper(I) Compounds .................................................. 83

Figure 4.3 The synthetic procedure for producing the tert-butyl-imino-2-

dimethylpyrrolidine ligand................................................................................................ 85

Figure 4.4 Structure of 1, shown with the hydrogens removed for clarity. The thermal

ellipsoids are at 30 %. ....................................................................................................... 86

Figure 4.5 Structure of (a) 3 and (b) 4, shown with the hydrogens removed for clarity.

The thermal ellipsoids are at 30 %. ................................................................................... 89

Figure 4.6 Thermal stress test of compounds (a) 3 showing no change in residual mass

with increasing sample mass, and (b) 1, showing increasing residual mass with increasing

initial sample mass. ........................................................................................................... 91

Figure 4.7 Thermal stress test trends for compounds 1–4. .............................................. 92

Figure 4.8 Evaporation kinetics of 1–4 by TGA. ............................................................. 93

Figure 4.9 Thermal decomposition of 1–4 in C6D6 at 165 °C over 21 days. ................... 94

Figure 4.10 Reactivity of 1 with silica: (a) shows the SS-13

C NMR of silica after

deposition of 1 at 275°C (top trace) compared to the HR-13

C NMR of 1 in deuterated

benzene (bottom trace). (b) shows the HR-1H NMR of the surface species etched from

the silica with D2O (in D2O; top trace) compared to the HR-1H NMR of 1 in CDCl3

(bottom trace). (c) shows the proposed nucleation and chemisorption of 1 at a silanol

group on a silica surface. .................................................................................................. 98

Figure 5.1 Amidinates, Guanidinates, and Iminopyrrolidinates Used as Ligands For

Precursors in CVD and ALD (R, R’ = any alkyl group). ............................................... 111

Figure 5.2 Synthesis of Silver(I) and Gold(I) tert-butyl-imino-2,2-dimethylpyrrolidinate.

......................................................................................................................................... 113

Figure 5.3 Molecular diagram of 2 with thermal ellipsoids at 30% probability. H-atoms

omitted for clarity. Ag analogue compound 1 is isomorphic with 2. ............................. 114

Figure 5.4 Thermogravimetric analysis of 1 (black) and 2 (gray). Experiments were run

under 1 atm of nitrogen with a ramp rate of 10 °C/min. Sample sizes for 1 and 2 were

10.49 mg and 13.65 mg, respectively. ............................................................................ 116

Figure 5.5 . Isothermal TGA of (a) 1 and (b) 2. The furnace was heated at 40 °C/min up

to the isothermal temperature. Isothermal temperatures are indicated in the right hand

legend (°C). Samples sizes were between 3.10 mg to 3.67 mg. ..................................... 117

Page 19: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

xix

Figure 5.6 Differential scanning calorimetry of 1, 2, and 3 in hermetically sealed

aluminum pans. Temperature ramp was 10 °C/min up to 325 °C. Sample masses were

1.066 mg, 1.625 mg, and 3.790 mg for 1, 2, and 3, respectively. Exotherms are up. .... 118

Figure 5.7 Evaporation kinetics of 1 (♦), 2 (■) and 3 (●). ............................................. 119

Figure 5.8 Decomposition of 1 and 2 in solution (C6D6) measured by 1H NMR. ......... 120

Figure 5.9 Film thickness determined from the CVD of 1 (bottom) and 2 (top) at

different furnace temperatures. Depositions with 1 consumed 50 mg - 60 mg of

compound. Depositions from 2 consumed varying amounts: 13.9 mg (300 °C); 21.8 mg

(350 °C); 5.9 mg (400 °C); 20.6 mg (450 °C); 23.5 (500 °C). ....................................... 121

Figure 5.10 SEM images for thin films deposited from (a, b) 1 and (c, d) 2 at 200 °C and

350 °C, respectively. Images from the CVD of 1 were measured (a) 0.75 cm and (b) 7.75

cm from the precursor inlet. Images from the CVD of 2 were measured (a) 5 cm and (b)

11 cm from the precursor inlet. ....................................................................................... 123

Figure 5.11 Film thickness determined from timed CVD experiments of 1 under a low

flow of N2 at 300 °C with a system pressure of 100 mtorr. ............................................ 125

Figure 5.12 XPS survey spectrum of Ag on Si(1 0 0) substrate as-deposited (blue), after

1 sputtering cycle (green), after 2 sputtering cycles (red), and after 3 sputtering cycles

(black). Ar+ sputtering cycles lasted 2 min and were done under base Ar pressures of 1 x

10-5

Torr. ......................................................................................................................... 134

Figure 5.13 XPS survey spectrum of Au on Si (1 0 0) substrate as deposited (black), after

1 sputtering cycle (red), after 2 sputtering cycles (green), after 3 sputtering cycles (blue),

and after 4 sputtering cycles (cyan). Ar+ sputtering cycles lasted 2 min and were done

under Ar pressures of 1 x 10-5

Torr. ................................................................................ 135

Figure 6.1 The structures of 1,3-diisopropyl-imidazolin-2-ylidene copper

hexamethyldisilazide (1) and 4,5-dimethyl-1,3-diisopropyl-imidazol-2-ylidene copper

hexamethyldisilazide (2). ................................................................................................ 142

Figure 6.2 Thermogravimetric analyses and evaporation rates of 1 (black) and 2 (grey)

run at 10 °C/min ramp rate, with 10 °C increments for the stepped isotherm used to

determine evaporation rate. ............................................................................................. 144

Figure 6.3 The X-ray structure of 1 (left) and 2, (right), with H-atoms and minor

disordered contributions omitted for clarity and at 30 % probability ellipsoids. ............ 145

Figure 6.4 ALD saturation curve for 1 as the pulse length of 1 was varied. ................. 148

Figure 6.5 Scanning electron micrographs of deposited copper films. (a) Plan view of

copper nanoparticles deposited using a 1 s pulse length. (b) Plan view of crystalline

Page 20: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

xx

copper deposited using a 4 s pulse length. (c) Plan view of crystalline copper deposited

using a 6 s pulse length. (d) A profile of crystalline copper deposited using a 6 s pulse

length............................................................................................................................... 149

Figure 6.6 Optimized geometries of (a) 2 molecularly physisorbed on a smooth Cu (111)

surface; (b) CuN(SiMe3)2 chemisorbed on the smooth surface; (c) NHC from 2

chemisorbed onto a rough surface; (d) NHC from 2 physisorbed on the smooth surface.

......................................................................................................................................... 151

Figure 7.1 Structural differences between 1,3-diisopropyl-imidazolin-2-ylidene copper

hexamethyldisilazide (5) and 4,5-dimethyl-1,3-diisopropyl-imidazol-2-ylidene copper

hexamethyldisilazide (3). ................................................................................................ 164

Figure 7.2 General Synthetic Conditions for 1-10. ........................................................ 166

Figure 7.3 Synthesis of 4,5-dimethyl-1,3-ditertbutyl-imidazolinium chloride. ............. 167

Figure 7.4 Molecular diagram of 7 (left) and 8 (right) with thermal ellipsoids at 30%

probability. H-atoms omitted for clarity. ........................................................................ 169

Figure 7.5 Imidazolylidenes and Imidazolinylidenes, N-heterocyclic Carbenes (NHC);

and the Formamidinylidenes, Acyclic Diamino Carbenes (ADC), Evaluated in

Monomeric Cu(I) HMDS Complexes 1-10. ................................................................... 171

Figure 7.6 Thermal gravimetric analysis of 2, 3, 5, and 9. Experiments were run under 1

atm nitrogen with a ramp rate of 10 °C/min. Sample sizes were between 5 – 7mg. ...... 172

Figure 7.7 Thermal Decomposition of [ItBu2]Cu(I)HMDS (2) via Deportonation of the

Unsaturated NHC Backbone and Elimination of Hexamethyldisilazane. ...................... 173

Figure 7.8 TGA thermal stress test for 3 – 10. The heating rate was 10 °C/min for each

experiment. The smallest sample sizes were 1.3 μmol (~5 mg) and the largest were 15.9

μmol (~ 60mg). ............................................................................................................... 175

Figure 7.9 Isothermal rates of vaporization for 3 – 10 under 1 atm of nitrogen. ........... 178

Figure 7.10 Isothermal TG experiment of compound 2. An isotherm at 110 °C was

maintained until mass loss was negligible, followed by heating at a rate of 10 °C/min. 189

Figure 7.11 TG experiments for the imidazolinylidene Cu(I) HMDS compounds 4 – 7

under 1 atm N2. The heating rate was 10 °C/min and sample masses were 4 – 6 mg. ... 190

Figure 7.12 TG experiments for the formamidinylidene Cu(I) HMDS compounds 8 – 10

under 1 atm N2. The heating rate was 10 °C/min and sample masses were 4 – 6 mg. ... 191

Page 21: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

xxi

Figure 7.13 TGA thermal stress test for compound 10 illustrating thermal decomposition.

The heating rate was 10 °C/min and sample masses are shown top right. ..................... 192

Page 22: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

xxii

Abbreviations

ADC – acyclic diamino carbenes

AFM – atomic force microscopy

ALD – atomic layer deposition

CDI – N,N’-diisopropylcarbodiimide

CMP – chemical mechanical polishing

CVD – chemical vapour deposition

DCP – dispersion-correcting potentials

DFT – density functional theory

DSC – differential scanning calorimetry

ECD – electrochemical deposition

EDS – energy dispersive X-ray spectroscopy

GC-MS – gas phase chromatography mass spectrometry

HMDS – hexamethyldisilazide

HR-NMR – high resolution nuclear magnetic resonance

NHC – N-heterocyclic carbenes

NMR – nuclear magnetic resonance

MI FTIR – matrix isolation fourier transform infrared spectroscopy

MS – mass spectrometry

PE-ALD – plasma enhanced atomic layer deposition

PVD – physical vapour deposition

P-XRD – powder X-ray diffraction

QMS – quadrupole mass spectrometer

Page 23: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

xxiii

RGA – residual gas analyzer

SEM – scanning electron microscopy

SS-NMR – solid state nuclear magnetic resonance

TEM – transmission electron spectroscopy

TGA – thermal gravimetric analysis

TOF MS – time of flight mass spectrometry

VTMS – vinyltrimetylsilane

XPS – X-ray photoelectron spectroscopy

Page 24: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

1

Introduction 1 Chapter:

Motivation for Copper Seed Layers 1.1

Copper replaced aluminum as the conductive material in integrated circuits due to

a lower resistivity and a higher resistance to electro-migration stress.1 The performance

figure of merit for an integrated circuit is its “RC” time delay which is defined by the

resistivity (R) of the conductive wires and the capacitance (C) of the insulating medium.2

The switch from aluminum to copper occurred once the density of features and

components impeded the speed and frequency at which electrical signals could be

transmitted. Moore’s law correctly predicted the doubling of transistors every two years

within an integrated circuit which has guided research and developments efforts.3 To

allow for the exponential increase of the transistor density the physical dimension of each

transistor was reduced. Moore’s law provided guidelines for the down scaling of

transistor components and the hierarchical wiring structure.4

The replacement of aluminum with copper required a major reversal of fabrication

techniques.5 Aluminum is easily patterned through metal etch processes due to the

volatility of aluminum chlorides and fluorides. Aluminum wires were etched from

sputtered thin films with no considerations required for the conformality of the metal

deposition process. After patterning of the aluminum film, the negative space was in-

filled with a low-k dielectric and chemical mechanical polishing (CMP) removes the

excess dielectric material. For copper, a metal etch process was not feasible due to the

low volatility of its metal halides; therefore, the Damascene and dual-Damascene

processes were developed.6 Conceptually, the Damascene processes are the reverse of the

aluminum metal etch process.7 A blanket dielectric film is patterned through

Page 25: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

2

photolithographic methods followed by infilling by electrochemical deposition of copper

(EDC).8 The success of a Damascene process relies on a conformal, highly conductive,

void free copper seed layer. Additionally, copper interconnects require a barrier and an

adhesion layer to prevent diffusion of the copper atoms into the dielectric material and

void formation due to electromigration.9 Currently, a TaN/Ta thin film deposited by

physical vapour deposition (PVD) techniques is used as a barrier and adhesion layer in

today’s integrated circuit production line.1 The copper seed layer is deposited by PVD, as

well. The conformality of these films within current aspect ratios across all levels of the

hierarchical wire structure has been acceptable.

Conformality and total thickness of the liner films need to be addressed as the size

regime moves towards the 10 nm technology node.1 Current advanced techniques deposit

barrier/adhesion layers which would account for 40 % of the total area of a trench at the

10 nm node. The barrier/adhesion materials have higher resistivity than copper and would

increase the overall wire resistance, which is undesirable. Additionally, the subconformal

profiles of liner materials deposited by PVD can result in voids and seam defects after

electrochemical deposition of copper. Atomic layer deposition (ALD) of all liner

materials is being investigated as a possible deposition technique for future technology

nodes. Adoption of an entirely new liner system is likely since it is often found that

material performance differs depending on the deposition technique. For example, the

barrier performance of PVD TaN films might not be reproducible by ALD TaN.10

Secondly, Ta cannot be deposited by a suitable ALD process which has led to the

proposition of Ru as an adhesion and seed layers for copper interconnects.11

Copper ALD

Page 26: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

3

processes and precursors continue to be a relevant research area for the continued

implementation of copper seed layers in the future of interconnect based devices.

Atomic Layer Deposition 1.2

ALD is a gas phase, thin film deposition technique that achieves highly conformal

coatings in a layer by layer manner.12

The success of an ALD process relies entirely on

the self-limiting nature of the precursors’ surface reactions. A minimum of two

precursors are required to achieve the characteristic growth rate of ALD which is

reported in units of angstroms per cycle (Å/cycle).13

Adsorption of the metal containing

precursor typically occurs through a chemisorption process. This step deposits a surface

species that is capable of blocking further uptake of gaseous precursor and is referred to

as a self-limiting monolayer. The second precursor reacts with the monolayer to deposit

the target material. In some cases, particularly for metal films, the second precursor plays

a crucial role in desorbing any remaining fragments to refresh the surface for the next

chemisorption step. Growth rates for ALD tend to be less than the thickness of a

monolayer (i.e. ~2 Å for a copper monolayer) of the target material due to bulky surface

species blocking nucleation sites. Growth rates larger than a monolayer of the target

material generally are characterized as having a chemical vapour deposition (CVD)

component which indicates a deviation from self-limited growth behavior.

Three main criteria outline the design of a copper precursor capable of meeting

the requirements for industrial application. These criteria centre on the precursor’s

volatility, thin film deposition chemistry, and chemical composition. The first two criteria

are temperature dependent preferably met at low temperatures to reduce potential issues

related to thermal stability and thin film morphology. The precursor needs to generate

Page 27: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

4

sufficient vapour pressure at a temperature where negligible decomposition or molecular

rearrangement occurs. Precursor chemisorption and reactivity of the surface species to

copper metal at appreciable surface coverages will enable an acceptable growth rate.

Lastly, the precursor molecule must not contain atoms that contaminate or degrade the

barrier and adhesion layers, increase the resistance of the copper interconnect, or

compromise the longevity of the microelectronic device.

Processes for ALD have benefitted greatly from precursors sourced from known

homoleptic compounds such as alkyl, alkoxide, amido and halides (for example;

Ti(OiPr)4, AlMe3, SiCl4, Ta(NMe2)5).

14 These compounds are well studied, readily

available for many elements and typically possess suitable vapour pressure due to their

low molecular masses. When determining an ALD process employing a known

compound as a precursor, a more focused study on the characteristics of film growth is

possible. Preferably, one need not consider if a precursor is remaining intact while being

transported to the reaction chamber. Similar homoleptic compounds of copper have not

been reported in ALD research primarily due to thermal instability and low vapour

pressure due to a high degree of oligomerization.

Copper Alkyl, Amido, and Alkoxide Complexes 1.3

Copper(I) alkyl complexes (CuR, R = Me, Et, Pr, nBu) can be generated by

reaction of copper(I) or (II) halides with lithium, Grignard, or zinc reagents.15,16,17

When

isolated as pure solids they are explosive, which necessitates storage at sub-zero

temperatures. The stability of copper(I) alkyl complexes in solution is solvent dependent

showing higher stability in coordinating solvents.15

Decomposition mechanisms via

homolectic cleavage of the copper-carbon bond18

or β-hydride elimination19

have been

Page 28: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

5

studied in complexes stabilized with nBu3P. Structural characterization of homoleptic

copper(I) alkyl complexes has been inhibited due to their highly unstable nature and

tendency to precipitate from reaction solvents. Copper(I) alkyl complexes likely adopt a

high order oligomeric structure which would account for their non-volatile nature despite

their having low molecular masses. Copper(II) alkyl complexes have only been described

as metastable species with synthetic attempts resulting in the isolation of Cu(I)

products.16

Copper(I) amide complexes are significantly more stable and have been

structurally and thermally characterised. CuNR2 (for example; R = Me, Et, nBu, SiMe3)

complexes can be generated through salt metathesis between copper halides and lithiated

amines20,21,22

or, by a very appealing route, prepared from primary and secondary amines

with use from copper(I) mesityl as an efficient metalation reagent.23

These complexes

have been characterised as exclusively tetramers in solution and the solid state. Each

copper atom is two coordinate with each amido ligand bridging two copper atoms in a

Cu4N4 eight-membered ring. This arrangement is common throughout the alkyl, amido,

and alkyloxy complexes for copper(I); however it is most persistent within the amido

category as these complexes do not readily react with external nucleophiles compared to

the alkyl or alkoxy complexes.21

This is perhaps indicative of a higher degree of donor

bonding from the nitrogen lone pair to each Cu atom pair.20

Studies support β-hydride

abstraction as a mechanism for thermal decomposition.23

Several copper(I) amide

complexes were decomposed in tetralin solutions heated between 90 – 140 °C producing

the decomposition products of copper metal, the parent amine and the corresponding

imine.

Page 29: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

6

[CuNR2]4 → Cu + HNR2 + NRRʹ ;where Rʹ = R - βH

Volatility has only been demonstrated for [CuN(SiMe3)]4 which is the most thermally

stable tetramer yet possesses the highest molecular weight.22

Copper(I) alkoxide complexes have demonstrated a large range of thermal

stability showing a dependence on structure.24

For example, [CuOMe]4 decomposes

explosively at room temperature25

while [CuOCMe3]4 is stable up to 170 °C.26

In

addition, copper(II) alkoxide complexes are sufficiently stable to be isolated and

characterised which is a notable difference compared to the missing copper(II) alkyl and

amide complexes.27,28,29

Synthesis of stable copper(I) alkoxides and all copper(II)

alkoxides can be accomplished by salt metathesis. The less stable copper(I) alkoxides

were synthesised using copper methyl or mesityl as metalation reagents with alcohols.24

Copper(I) alkoxide complexes decompose to produce metallic copper via β-hydride

abstraction or copper-oxygen bond homolysis depending on the structure of the

alkoxide.24

Mechanisms for decomposition of copper(II) complexes have not been

thoroughly investigated, but results indicate the an opposite structural dependence on

thermal stability is observed compared to copper(I).28

Notably, disproportionation of

copper(I) to (II) has not been observed for the alkoxides. In fact, decomposition of

copper(II) alkoxides generate the copper(I) compounds when this is an adequately stable

species.26

Oxidation (by oxygen or peroxides) of copper(I) alkoxides to copper(II) is

possible.24,26

CVD of copper metal films from [CuOCMe3]4 has been demonstrated at

deposition temperatures of 400 °C under a system pressure of 10-5

Torr.30

The precursor

vapours are generated at 100 °C. Polycrystalline films were deposited without a reducing

agent and contained 5 % oxygen and <1 % carbon impurities consistent with the

Page 30: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

7

proposed mechanism of Cu-O bond homolysis. Copper(II) alkoxide complexes are

polymeric29

and non-volatile28

and not useful as precursors.

Copper(I) Chloride 1.4

Copper halides are insoluble solids possessing extended polymeric structures.

Melting points for all the halide compounds of both oxidation states are around 500 °C

and boiling points well above 1000 °C often associated with decomposition. Surprisingly,

copper(I) chloride has been used to test whether copper halides are suitable as precursors

for ALD. Copper(I) chloride generates sufficient vapour pressure when heated to 390 at

10 mbar. The major gaseous species is Cu3Cl3.31

Due to the necessary high temperatures

required to evaporate copper chloride the deposition temperature is restricted to higher

substrate temperatures which led to complicated surface chemistry straying from ideal

ALD behavior. These ALD studies were carried out on Al2O332

and Ta33

substrates using

elemental zinc and molecular hydrogen as reducing agents, respectively. Prior to the

experiments, the leading concern for depositing copper metal films with zinc was the

likely dissolution of zinc into copper forming a brass alloy. Dissolution of zinc occurred

and proved problematic due to its slow outgassing from the surface which continued

throughout the purging and following copper chloride pulse.32

This led to both precursors

interacting in the gas phase which caused a large film gradient across the furnace and also

high growth rates indicative of a CVD component to film growth. Results from ALD

work testing Ta substrates showed that a film of copper metal 30 to 40 nm could be

deposited without H2 pulses due to the reduction of CuCl by the substrate to form

thermodynamically favoured tantalum chloride species (corroborated by XPS analysis).33

Beyond the 30 – 40 nm of film deposition, the reduction of CuCl surface species by

Page 31: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

8

hydrogen was the rate determining step and required an estimated activation energy of 80

kJ/mol. Saturated growth behavior during the H2 pulse was not achieved even with pulse

lengths greater than 20 s.

Copper Precursors for Atomic Layer Deposition 1.5

Copper complexes of bidentate ligands have shown greater success as precursors

for CVD and ALD. The copper(II) complexes adopt square planar or distorted tetrahedral

geometry and the copper(I) complexes are typically dimeric when homoleptic with the

copper atom in a two-coordinate, linear geometry. Many copper(I) compounds can be

stabilised by Lewis bases as monomers where the bidentate ligand chelates the copper

atom in a three or four-coordination environment depending on the Lewis base.

Monomeric copper(I) complexes have been of interest in recent years due to their

facile disproportionation reaction to copper(II) and copper metal.34

Research efforts were

focused on controlling physical properties (eg. melting point, viscosity, solubility) to

maximize precursor delivery into a CVD chamber via direct liquid injection and, also, to

control the temperature of the disproportionation reaction which is important to obtain the

high purity films with resistivities within 10 % of bulk copper.35

The precursors that

received most of the attention were acetylacetonate (acac) copper(I) complexes stabilized

by soft bases such as alkenes and alkynes.36

Various substitution patterns of the acac

ligand at the 1- and 5- positions with alkyl or fluoro groups were studied and resulted in

control of physical properties and also affected the bonding around the copper center.37

For example, a higher degree of fluorination of the acac ligand decreased the electron

density at the copper center and strengthened the copper-Lewis base bond. Many Lewis

bases were studied to increase the bond strength towards copper.36

Dissociation of the

Page 32: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

9

Cu(I)-L bond could lead to decomposition of the precursor in its source container or

clogging of the direct-liquid-injection instrumentation which was undesirable.35

The

electron donating ability of the Lewis base could be increased by attaching electron

donating groups such as silyl groups38

or a conjugated unsaturated bond.36

A small

consequence of varying the substitution of the Lewis base was control over the initial

steps leading to precursor chemisorption;37

however, ultimately the rate limiting step to

copper metal deposition was the surface disproportionation reaction.39

The success of

these precursors in the CVD of high purity copper films at low temperatures meant that

they could not be precursors for ALD.

1.5.1 Cu KI5

A series of monomeric copper(I) complexes were prepared and studied to

overcome the limited applicability of precursors stabilised by vinyltrimethylsilyl (vtms)

to only CVD processes. In these complexes, the Lewis base (i.e. vtms) was tethered to the

anionic ligand (Figure 1.1). For this to be feasible the acetylacetonate framework required

substitution of at least one of the oxygen atoms to nitrogen, thus changing the

acetylacetonate to a ketoiminate or a dikitiminate.

Figure 1.1 The copper ketoiminate precursor CuKI5 with a tethered vinyl-silyl Lewis

base.

Page 33: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

10

The tethered VTMS group coordinated intramolecularly to the copper atom forming a

seven-membered ring and prevented thermal loss of the VTMS group inhibiting

disproportionation. As a result, these precursors could be heated to higher temperatures

generating higher vapour pressure without decomposition. For example, these complexes

have vapour pressures above 2 Torr at 140 °C while the untethered analogues will

decompose when heated in attempts to achieve similar vapour pressures.40

The initial

report on these complexes included experiments demonstrating behavior characteristic of

ALD precursors, except no saturation curves were collected.41

Growth rates varied

between 0.1 - 0.9 Å/cycle inside a temperature window of 150 – 200 °C which possibly

indicates a CVD film growth component due to the lack of a steady ALD growth

window. Later reports demonstrated promising results for these complexes as CVD

precursors in conjunction with formic acid as the reducing agent.42

These precursors were

not expected to deposit copper via a disproportionation mechanism; therefore, in theory,

total precursor consumption was being achieved. Recent surface studies of adsorbed

precursor monolayers on a Cu(110) single-crystal concluded that the tethered VTMS

group dissociated from the copper(I) atom upon chemisorption. Additionally, some

evidence for a copper(II) ketoiminate species was observed which indicated a small

component of disproportionation chemistry occurring for adsorbed CuKI5.43

1.5.2 Bis(tri-n-butylphosphine) Copper(I) acetylacetonate

An ALD process was achieved from a monomeric Cu(I) complex employing

(nBu3P)2Cu(acac) as a precursor. The bis-phosphine formulation is more thermally stable

towards disproportionation than their mono-phosphine analogues.44

This complex does

not possess the high volatility common amongst monomeric copper(I) precursors and has

Page 34: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

11

a vapour pressure behavior comparable to copper(II) acetylacetonate; however, it is a

liquid under standard conditions and can be delivered via direct-liquid-injection. The

ALD process was developed for thin films of Cu2O and used wet O2 as a co-reactant at

temperatures between 100–135 °C on a variety of substrates (Ta, Ru, TaN, SiO2).45

Surprisingly, despite the molecule’s saturated coordination sphere it chemisorbed at low

temperatures via dissociation of both phosphines.46

A narrow ALD window was

discovered adjacent to the onset of surface disproportionation and had a growth rate of

0.1 Å/cycle. The Cu2O thin films were subsequently reduced under formic acid flow at

110-120 °C to be used as seed layers for electrochemical copper deposition.

1.5.3 Copper(II) acetylacetonate precursors

Many copper(II) complexes have also been studied as viable precursors for ALD.

With these precursors, disproportionation is not a concern; however, they tend to require

high temperatures or strong reducing agents to obtain metallic films. For example,

copper(II) acetylacetonate (Figure 1.2) has been employed in ALD processes using

molecular hydrogen and hydrogen radicals at temperatures of 250 °C47

and between 85-

140 °C,48,49

respectively. This difference in temperatures highlights how reactivity of

chemisorbed Cu(II) precursors are a more relevant concern rather than precursor

adsorption. Surface studies of copper(II) acetylacetonate on Ni(110) and Cu(110) single

crystals concluded that reduction of the precursor ion occurs for adsorbed molecules near

room temperature and that the role of the second precursor is to remove the remaining

organic molecules.50

Page 35: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

12

Figure 1.2 Copper(II) acetylacetonate, R = H; tetramethylheptanedionate, R = Me;

hexafluoroacetylacetonate, R = F.

Two variants of copper(II) acetylacetonate have been studied in ALD processes.

Copper(II) hexafluoroacetylacetonate (hfac) and copper(II) tetramethylheptanedionate

(tmhd) are advantageous due to higher volatility51

and higher thermal stability,

respectively (Figure 1.2). A wide deposition temperature window is possible for

copper(II) hfac due to a low sublimation temperature. Alcohols and formaldehyde were

used as reducing agents at temperatures of 230–300 °C showing a high growth rate of 2.2

Å/cycle, for which, the self-limiting nature was not confirmed.52

These high temperatures

were necessary due to the choice of reducing agents. Half cycles for film nucleation at

considerably lower temperatures is feasible. Stable monolayers of copper(II) hfac

adsorbed onto Al2O3 have been studied at substrate temperatures of 80 °C.53

Hydrogen

plasma was used to complete the full ALD cycle. Additonally, room temperature

reduction of adsorbed copper(II) hfac on TiN substrates by molecular hydrogen catalysed

by pyridine has been demonstrated.54

The growth rate from 25–100 °C was 0.18 Å/cycle

and the films contained significant oxygen and carbon impurities.

ALD work based on copper(II) thmd have focused on the selective deposition of

copper metal on Pd or Pt seed layers using molecular hydrogen at substrates temperatures

of 135–260 °C.55

The initial surface mechanism was believed to involve Pd/Pt catalysed

Page 36: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

13

reduction of the copper(II) tmhd monolayer during the hydrogen pulse; however, recently

it has been shown that adsorption of copper(II) tmhd is readily reversible during the

purging steps of the ALD cycle.56

The surface interaction of the two precursors occurs

because the Pd seed layer retains dissociated hydrogen until the following copper(II)

tmhd pulse. Intermixing of the Cu layer with the Pd seed layers also occurred and led to a

surface presence of Pd which could continually participate in the uptake of hydrogen as

the copper film accumulated.57

Reversible adsorption of copper(II) thmd was not a

concern when metal nitrides, metal oxides or metals with low activity towards hydrogen

are used as substrates since ALD using hydrogen plasma as a co-reactant has been

demonstrated on SiO2, Au, and TaNx between 90 to 250 °C. 58

1.5.4 Copper(II) diketoiminate precursors

Copper(II) ketoiminates are compelling alternatives to the diketonates. The lower

oxygen content of the ketoiminate ligand is advantageous for metal depositions and the

variability of the N-substituent can be used to tune the physical characteristics of the

precursor and process conditions.59

Due to the added steric bulk of the N-substituents the

solid state structures of copper(II) ketoiminates adopt distorted square planar or

tetrahedral geometry.60

The diketonates are flat, square planar molecules that efficiently

stack in the solid state. Consequently, copper(II) ketoiminates have higher volatility and

Figure 1.3 Copper(II) 2-ethylimino-4-pentanonate

Page 37: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

14

low melting points as a result of the disrupted intermolecular interaction.61

Copper metal

films have been deposited employing copper(II) 4-ethyimino-pentan-2-one (Figure 1.3)

and molecular hydrogen as a co-reactant at deposition temperatures between 120–220 °C

on Pt and Ru substrates.62

Growth rates of 1.2 - 1.7 Å/cycle were reported without data

confirming self-limited growth. The main focus was the sheet resistance of the copper

films. Sheet resistance was found to be dependent on deposition temperature due to

changes in film morphology. Plasma enhanced ALD was also possible within a

temperature window of 30 – 100 °C.61

Even though the precursor was evaporated at 85

°C the growth rates and precursor pulse length did not indicate precursor transport or

condensation to be a concern. Self-limited growth was confirmed and a growth rate of 0.3

Å /cycle was observed. With preferentially oriented Ru(001) thin film substrates, smooth

and continuous Cu(111) oriented films are obtained which are desirable features for seed

layers in the electrodeposition of copper.63

Evidently, complete in-filling of high aspect

ratio trenches was demonstrated for a 13 nm Cu seed layer using the low-temperature

plasma enhanced process.61

1.5.5 Copper(I) and (II) dikitiminate precursors

Substitution of both oxygen atoms for nitrogen of the diketonate ligand affords

the diketiminate ligand for which copper(I) and (II) complexes have been studied as

Figure 1.4 Asymmetric copper(I) and (II) dikitiminate precursors.

Page 38: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

15

precursors (Figure 1.4).64,65

The ligand framework is highly amenable to symmetric and

unsymmetric variation of four alkyl groups including cyclization of a nitrogen atom to

the ligand backbone. In comparison to the diketonate and ketoiminate copper complexes,

the diketiminates are more volatile which can be attributed to their distorted tetrahedral

geometries, dissymmetry and alkyl substitutions.64-66

Pulsed CVD was demonstrated for a

monomeric copper(I) diketiminate at deposition temperatures of 120 °C which required a

silane as a co-reactant to achieve films with low levels of contaminants.67

Deposition

temperatures could be lowered to 45 °C if pyrazole was adsorbed to the surface prior to

passing the copper precursor over the substrate; however, a self-limiting growth behavior

was not confirmed and film thickness was dependent on precursor pulse.68

There is

limited data regarding use of a copper(II) diketiminate precursors to grow copper thin

films. Considering their superior volatility, a low temperature plasma enhanced process

similar to the reports for copper(II) diketoiminates would be promising.

1.5.6 Copper(I) amidinate precursors

Copper(I) amidinate complexes are a unique class of copper ALD precursor that

do not undergo the detrimental copper(I) disproportionation reaction.69

These complexes

share similarities to copper(I) amide complexes; however possess desirable properties of

thermal stability and volatility. Like the copper(I) amides, the copper(I) amidinates are

Figure 1.5 Copper(I)-N,Nʹ-di-sec-butylacetamidinate

Page 39: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

16

nitrogen donor ligands with linear coordination geometry around each copper center

(Figure 1.5). They are only stable in the copper(I) oxidation state. Typically, a dimeric

structure is obtained with a highly symmetric metallocycle containing approximately

equivalent Cu-N and C-N bond lengths due to the resonant imine bond of the amidinate

ligand. The amidinate ligands provide a high degree of steric protection of the

coordinated copper centers using bulky aliphatic groups that allow only weak

intermolecular interactions. Along with the strong bond between copper and nitrogen,

these complexes generate appreciable vapour pressures when heated. Copper metal films

have been deposited on a variety of substrates at deposition temperature of 150–190°C

using molecular hydrogen as a co-reactant.70

Oxynitride,71

nitride,72

and sulphide73

films

can be deposited at temperatures above 130°C with self-limited film growth. Surface

studies on silica surfaces have shown chemisorption proceeding through displacement of

one amidinate ligand by a surface hydroxyl group.74

The remaining surface amidinates

are removed following the hydrogen pulse. On metallic surfaces, a monolayer of

chemisorbed precursor exists as reduced copper atoms and dehydrogenated ligand

fragments.75

The primary role of the hydrogen pulse is to desorb any ligand fragments

and not to reduce the deposited copper atom. The processes developed for copper(I)

amidinate complexes provide suitable seed layers76

and impressive means to completely

in-fill narrow trench features employing a surface activation agent.77

1.5.7 Copper(II) aminoalkoxide precursors

Copper(II) aminoalkoxides were developed to fill the void of copper alkoxides in

copper precursors. These monomeric precursors have square planar geometry stabilised

Page 40: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

17

by an amino group tethered to each alkoxide (Figure 1.6).78

Similar to the simple

copper(II) alkoxides,

Figure 1.6 Copper(II) aminoalkoxides, R = H, alkyl, fluoroalkyl.

the aminoalkoxides can undergo thermal decomposition via β or γ-hydride abstraction

and afford pure copper metal films above 200 °C in CVD processes.79,80

Fortunately,

these complexes show high volatility even without fluorinated ligands81

and several low

temperature ALD processes have been developed. A thermal ALD study employing

molecular hydrogen as the co-reactant on Ru substrates found low film nucleation and

growth rates within the viable temperature window of the precursor.82

In the same work,

copper seed layers were more easily fabricated through a thermal copper nitride ALD

process between 100-140 °C followed by reduction at 200 °C. Plasma enhanced ALD has

been reported for two copper(II) aminoalkoxide precursors.63,83

Deposition temperatures

down to 30 °C and up to the decomposition temperature of the specific copper(II)

aminoalkoxide (i.e. >160 °C) were studied and growth rates were measured to be 0.2 –

0.6 Å/cycle. The copper metal films deposited at low temperatures are smooth and

consist of dense, connected particles with a crystalline texture strongly influenced by that

of the substrate.63

Film impurities increased for films deposited at low substrate

temperatures due to inefficient desorption of ligand fragments which resulted in film

resistivity higher than bulk copper. Copper(II) aminoalkoxide complexes have also been

Page 41: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

18

studied in combination with unconventional co-reactants to achieve low-temperature

copper deposition without plasma generated atomic hydrogen. Volatile alkylation

reagents are particularly useful for copper metal ALD due to facile ligand exchange

reactions and the instability of copper alkyl complexes.84

For example, copper(II)

dimethylamino-2-propoxide and diethyl zinc were used as co-reactants to deposit copper

metal films between 100-120 °C at a self-limiting growth rate of 0.2 Å/cycle.85

The ALD

temperature window was narrow in order to limit film impurities. Lower temperatures

decreased desorption of the Zn products resulting from the ligand exchange surface

reactions and high temperatures caused decomposition of the diethyl zinc co-reactant.

Strong reducing agents such as hydrazine86

or amino boranes87

are also suitable co-

reactants capable of copper metal ALD near 100 °C. These reducing agents have optimal

performance when used along with formic acid and/or a metal catalyst to assist the

reduction chemistry.

1.5.8 Copper Precursor Summary

The shortcomings of alkyl, amido and alkoxide homoleptic copper compounds is

mitigated by a vast library of suitable chelation complexes available for copper CVD and

ALD processes. Very few examples of copper(I) precursors are available for ALD

because the minimum temperature for disproportionation reactions precedes the

minimum adsorption temperature. As a general guideline, if copper(I) and (II) oxidation

states exist for a given ligand class then only the copper(II) compounds will be useful

ALD precursors. Copper(I) amidinates are, so far, the best preforming copper(I)

precursor. The ALD window for copper metal films has been limited by the activity of

molecular hydrogen. Plasma-enhanced ALD or thermal ALD with a novel co-reactant

Page 42: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

19

may yield low temperature results for the amidinate precursors. The evolution of the

copper(II) precursor has traversed step-by-step from chelating oxygen ligands forming

six membered metallo-cycles to chelating nitrogen ligands forming five-membered

metallo-cycles. The progression was fueled by improvements in volatility due to, in part,

changes in coordination geometry and was accompanied by losses in thermal stability.88

Copper metal deposition by thermal ALD from copper(II) precursors has been reported

between 100-250 °C. The lower temperature limit depends on the activity of molecular

hydrogen with the substrate and the upper limit depends on the stability of the precursor.

Novel co-reactants have widened the ALD window by lowering the minimum deposition

temperature. Plasma-enhanced processes seem to have bottomless windows given the

precursor is sufficiently volatile. Processes and formulations for new copper (I) and (II)

precursors will continue to be explored. For example, additional ALD studies for

copper(II) pyrrolylaldiminates are expected to be reported.84

Also, heteroleptic copper(II)

compounds have recently appeared in the academic89

and patent90

literature. ALD studies

should be forthcoming.

Upcoming Thesis Chapters 1.6

This thesis can be divided into two parts about separate research programs dealing

with developing copper precursors. The first begins with a ligand modification to

amidinates and proceeds through numerous thermolysis studies ending with an improved

ligand design and thermally robust precursors for group 11 metals. Briefly, Chapter 2

describes the synthesis and thermal characterisation of copper(I) guanidinate compounds

followed by their use as precursors for copper metal films without requiring a reducing

agent. Comparative experiments for a copper(I) amidinate were performed and the

Page 43: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

20

differences are discussed with respect to a particular decomposition mechanism, CDI de-

insertion. Chapter 3 involves an investigation with advanced techniques to determine β-

hydride abstraction as the gas phase thermal decomposition mechanism of a copper(I)

guanidinate compound. Previously, iminopyrrolidinate ligands were developed in our

group to eliminate CDI-deinsertion as a mechanism of decomposition. In Chapter 4, a

modified iminopyrrolidine which also prevents β-hydride abstraction is described.

Chapter 4 and 5 details a comparison of several copper(I) iminopyrrolidinates, as well as,

silver(I) and gold(I) iminopyrrolidinates to highlight the improved ligand design.

The second part of this thesis introduces diamino carbenes (e.g. NHC) to the

library of ligands available for designing copper precursors. Motivation came from the

lack of monomeric copper(I) amidinate, guanidinate, and iminopyrrolidinate complexes

in the literature. Stable carbenes were used to break their dimeric structure; however, the

monomers were less volatile and less stable. Chapter 6 entails two monomeric copper(I)

amide precursors employing two different NHCs and their use in PE-ALD of copper

metal films. The differences in their ALD chemistry could only be attributed to the

differences in the NHCs. Chapter 7 explores a large series of cyclic and acyclic diamino

carbenes and how their differences affect precursor properties.

References1.7

1 2013 Edition of the International Technology Roadmap for Semiconductors;

http://www.itrs.net/Links/2013ITRS/2013Chapters/2013Interconnect_Summary.pdf.

2 Havemann, R. H.; Hutchby, J. A. Proceedings of the IEEE 2001, 89, 586 – 601.

3 Moore, G. E. Electronics, 1965, 114-117.

Page 44: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

21

4 Theis, T. N. IBM J. Res. Develop. 2000, 44, 379-390.

5 Gambino, J.; Chen, F.; He, J. Custom Integrated Circuits Conference 2009, 141, 13-

16.

6 Andricacos, P. C.; Uzoh, C.; Dukovic, J. O.; Horkans, J.; Deligianni, H. IBM J. Res.

Develop. 1998, 42, 567-574.

7 Merchant, S. M.; Kang, S. H.; Sanganeria, M.; Schravendijk, B. v.; Mountsier, T.

JOM 2001, 53, 43-48.

8 Gambino, J. P. ECS Transactions 2011, 35, 687-699.

9 Kaloyeros, A. E.; Eisenbraun, E. Annu. Rev. Mater. Sci. 2000, 30, 363-385.

10 Wojcik, H.; Friedmann, M.; Feustel, F.; Albert, M.; Ohsiek, S.; Metzger, J.; Voss, J.;

Bartha, J. W.; Wenzel, C. IEEE Int. Interconnect Techology Conf. 2007, 19-21.

11 Yang, C.-C.; Spooner, T.; Ponoth, S.; Chanda, K.; Simon, A.; Lavoie, C.; Lane, M.;

Hu, C.-K.; Liniger, E.; Gignac, L.; Shaw, T.; Cohen, S.; McFeely, F.; Edelstein, D.

IEEE Int. Interconnect Techology Conf. 2006, 187-189.

12 George, S. M. Chem. Rev. 2010, 110, 111-131.

13 Li, W.-M. Chem. Vap. Dep. 2013, 19, 82-103.

14 Miikkulainen, V.; Leskela, M.; Ritala, M.; Puurunen, R. L. J. Appl. Phys. 2013, 113,

021301.

15 Bertz S. H.; Dabbagh, G. Tetrahedron 1989, 45, 425-434.

16 Wada, K.; Tamura, M.; Kochi, J. J. Am. Chem. Soc. 1970, 92, 6656-6658.

17 Thiele, K.-H.; Kohler, J. J. Organometallic Chem. 1968, 12, 225-229.

18 Whitesides, G. M.; Panek, E. J.; Stedronsky, E. R. J. Am. Chem. Soc. 1972, 94, 232-

239.

19 Whitesides, G. M.; Stedronsky, E. R.; Casey, C. P.; Filippo, J. S. J. Am. Soc. Chem.

1970, 92, 1426-1427.

20 Hope, H.; Power, P. P. Inorg. Chem. 1984, 23, 936-937.

Page 45: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

22

21 Gambarotta, S.; Bracci, M.; Floriani, C.; Chiesi-Villa, A.; Guastini, C. J. Chem. Soc.

Dalton. Trans. 1987, 1883-1888.

22 James, A. M.; Laxman, R. K.; Fronczek, F. R.; Macerick, A. W. Inorg. Chem. 1998,

37, 3785-3791.

23 Tsuda, T.; Watanabe, K.; Miyata, K.; Yamamoto, H.; Saegusa, T. Inorg. Chem.

1981, 20, 2728-2730.

24 Whitesides, G. M.; Sadowski, J. S.; Lilburn, J. J. Am. Chem. Soc. 1974, 96, 2829-

2835.

25 Costa, G.; Camus, A.; Marsich, N. J. Inorg. Nucl. Chem. 1965, 27, 281-285.

26 Tsuda, T.; Toshiaki, H.; Saegusa, T. J. Am. Chem. Soc. 1972, 94, 658-659.

27 Brubaker, C. H.; Wicholas, M. J. Inorg. Nucl. Chem. 1965, 27, 59-62.

28 Singh, J. V.; Baranwal, B. P.; Mehrotra, R. C. Z. anorg. allg. Chem. 1981, 477, 235-

240.

29 Nelson, K. J.; Guzei, I. A.; Lund, G. S.; McGaff, R. W. Polyhedron 2002, 21, 2017-

2020.

30 Jeffries, P.; Girolami, G. S. Chem. Maters. 1989, 1, 8-10.

31 Brewer, L.; Lofgren, N. L. J. Am. Chem. Soc. 1950, 72, 3038.

32 Juppo, M.; Ritala, M.; Leskelä, M. J. Vac. Sci. Technol. A 1997, 15, 2330-2333.

33 Mårtensson, P.; Carlsson, J.-O. Chem. Vap. Dep. 1997, 3, 45-50.

34 Hampden-Smith, M. J.; Kodas, T. T. Polyhedron 1995, 14, 699-732.

35 Petersen, G. A.; Parmeter, J. E.; Apblett, C. A.; Gonzales, M. F.; Smith, P. M.

Omstead, T. R.; Norman, J. A. T. J. Electrochem. Soc. 1995, 142, 939-944.

36 Doppelt, P. Coord. Chem. Rev. 1998, 178-180, 1785-1809.

37 Chen, T.-Y.; Vaissermann, J.; Ruiz, E.; Senateur, J. P.; Doppelt, P. Chem. Mater.

2001, 13, 3993-4004.

38 Tran, P. D.; Doppelt, P. Surf. Coat. Technol. 2007, 201, 9066-9070.

Page 46: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

23

39 Girolami, G. S.; Jeffries, P. M.; Dubois, L. H. J. Am. Chem. Soc. 1993, 115, 1015-

1024.

40 Norman, J. A. T.; Perez, M.; Schulz, S. E.; Waechtler, T. Microelectronic

Engineering 2008, 85, 2159-2163.

41 Norman, J. A. T.; Perez, M.; Lei, X.; Cheng, H. ECS Transactions 2007, 3, 161-170.

42 Song, H.; Norman, J. A. T.; Shimogaki, Y. Microelectronic Engineering 2010, 87,

249-253.

43 Ma, Qiang, Zaera, F. J. Vac. Sci. Technol. A 2015, 33, DOI: 10.1116/1.4896940

44 (a) Shin, H.-K.; Hampden-Smith, M. J.; Duesler, E. N.; Kodas, T. T. Polyhedron,

1991, 10, 645-647, (b) Shin, H.-K.; Hampden-Smith, M. J.; Duesler, E. N.; Kodas, T.

T. Can. J. Chem. 1992, 70, 2954-2966.

45 Waechtler, T.; Ding, S.-F.; Hofmann, L.; Mothes, R.; Xie, Q.; Oswald, S.;

Detavernier, C.; Schulz, S. E.; Qu, X.-P.; Lang, H.; Gessner, T. Microelectronic

Engineering 2011, 88, 684-689.

46 Dhakal, D.; Waechtler, T.; Schulz, S. E.; Gessner, T.; Lang, H.; Mothes, R.;

Tuchscherer, A. J. Vac. Sci. Technol. A 2014, 32, 041505.

47 Utriainen, M.; Kroger-Laukkanen, M.; Johansson, L.-S.; Niinisto, L. Appl. Surf.

Sci.2000, 157, 151-158.

48 Niskanen, A.; Rahtu, A.; Sajavaara, T.; Arstila, K.; Ritala, M.; Leskela, M. J.

Electrochem. Soc. 2005, 152, G25-G28.

49 Wu, L.; Eisenbraun, E. J. Vac. Soc. Technol. B 2007, 25, 2581-2585.

50 Qiang, M.; Zaera, F. J. Vac. Sci. Technol. A 2013, 31, 01A112.

51 Fahlman, B. D.; Barron, A. R. Adv. Mater. Opt. Electron. 2000, 10, 223-232.

52 Solanki, R.; Pathangey, B. Electrochem. Solid-State Lett. 2000, 3, 479-480.

53 Chaukulkar, R. P.; Thissen, N. F. W.; Rai, V. R.; Agarwal, S. J. Vac. Sci. Technol. A

2014, 32, 01A108.

54 Kang, S.-W.; Yun, J.-Y.; Chang, Y. H. Chem. Mater. 2010, 22, 1607-1609.

55 Martensson, P.; Carlsson, J.-O. J. Electrochem. Soc. 1998, 145, 2926-2931.

Page 47: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

24

56 Jiang, X.; Wang, H,; Qi, J.; Willis, B. G. J. Vac. Sci. Technol. A. 2014, 32, 041513.

57 Hsu, I. J.; McCandless, B. E.; Weiland, C.; Willis, B. G. J. Vac. Sci. Technol. 2009,

27, 660-667.

58 Jezewski, C.; Lanford, W. A.; Wiegand, C. J.; Singh, J. P.; Wang, P.-I.; Senkevich, J.

J.; Lu, T.-M. J. Electrochem. Soc. 2005, 152, C60-C64.

59 Stabnikov, P. A. Russ. J. Gen. Chem. 2013, 83, 1919-1927.

60 Baidina, I. A.; Stabnikov, P. A.; Vasiliev, A. D.; Gromilov, S. A.; Igumenov, I. K. J.

Struct. Chem. 2004, 45, 671-677.

61 (a) Mao, J.; Eisenbraun, E.; Omarjee, V.; Korolev, A.; Dussarrat, C. ECS

Transactions 2011, 35, 125-132, (b) Mao, J.; Eisenbraun, E.; Omarjee, V.; Korolev,

A.; Dussarrat, C. IEEE Trans. Semicond. Manuf. 2013, 26, 17-22.

62 (a) Park, K.-M.; Kim, J.-K.; Han, B.; Lee, W.-J.; Kim, J.; Shin, H.-K.

Microelectronic Engineering 2012, 89, 27-30, (b) Han, B.; Park, K.-M.; Park, K.;

Park, J.-W.; Lee, W.-J. IEEE Int. Interconnect Techology Conf.2009, 173-174.

63 Hagen, D. J.; Connolly, J.; Nagle, R.; Povey, I. M.; Rushworth, S.; Carolan, P.; Ma,

P.; Pemble, M. E. Surf. Coat. Technol. 2013, 230, 3-12.

64 Park, K.-H.; Bradley, A. Z.; Thompson, J. S.; Marshall, W. J. Inorg. Chem. 2006, 45,

8480-8482.

65 Park, K.-H.; Marshall, W. J. J. Am. Soc. Chem. 2005, 127, 9330-9331.

66 Morozo, N. B.; Stabinokov, P. A.; Baidina, I. A.; Semyannikov, P. P.; Trubin, S. V.;

Igumenov, I. K. J. Struct. Chem. 2007, 48, 889-898.

67 Thompson, J. S.; Zhang, L.; Wyre, J. P.; Brill, D. J.; Lloyd, K. G. Thin Solid Films

2009, 517, 2845-2850.

68 Thompson, J. S.; Zhang, L.; Wyre, J. P.; Brill, D.; Li, Z. Organometallics 2012, 31,

7884-7892.

69 Li, Z.; Barry, S. T.; Gordon, R. G. Inorg. Chem. 2005, 44, 1728-1735.

70 Li, Z.; Rahtu, A.; Gordon, R. G. J. Electrochem. Soc. 2006, 153, C787-C794.

Page 48: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

25

71 Kim, H.; Bhandari, H. B.; Xu, S.; Gordon, R. G. J. Electrochem. Soc. 2008, 155,

H496-H503.

72 Li, Z.; Gordon, R. G. Chem. Vap. Dep. 2006, 12, 435-441.

73 Martinson, A. B. F.; Elam, J. W.; Pellin, M. J. Appl. Phys. Lett. 2009, 94, 123107.

74 Dai, M.; Kwon, J.; Halls, M. D.; Gordon, R. G.; Chabal, Y. J. Langmuir 2010, 26,

3911-3917.

75 (a) Ma, Q.; Guo, H.; Gordon, R. G.; Zaera, F. Chem. Mater. 2010, 22, 352-359, (b)

Ma, Q.; Guo, H.; Gordon, R. G.; Zaera, F. Chem. Mater. 2011, 23, 3325-3334, (c)

Ma, Q.; Zaera, F.; Gordon, R. G. J. Vac. Soc. A 2012, 30, 01A114.

76 Li, Z.; Gordon, R. G.; Farmer, D. B.; Lin, Y. Vlassak, J. Electrochem. Solid-State

Lett. 2005, 8, G182-G185.

77 Au, Y.; Lin, Y.; Gordon, R. G. J. Electrochem. Soc. 2011, 158, D248-D253.

78 Goel, S. C.; Kramer, K. S.; Chiang, M. Y.; Buhro, W. E. Polyhedron 1990, 9, 611-

613.

79 Becker, R.; Devi, A.; Wei, J.; Weckenmann, U.; Winter, M.; Keiner, C.; Becker, H.-

W.; Fischer, R. A. Chem. Vap. Dep. 2003, 9, 149-156.

80 Park, J. W.; Jang, H. S.; Kim, M.; Sung, K.; Lee, S. S.; Chung, T.-M.; Koo, S.; Kim,

C. G.; Kim, Y. Inorg. Chem. Commun. 2004, 7, 463-466.

81 Chi, Y.; Hsu, P.-F.; Liu, C.-S.; Ching, W.-L.; Chou, T.-Y.; Carty, A. J.; Peng, S.-M.;

Lee, G.-H.; Chuang, S.-H. J. Mater. Chem. 2002, 12, 3541-3550.

82 Park, J.-M.; Jin, K.; Han, B.; Kim, M. J.; Jung, J.; Kim, J. J.; Lee, W.-J. Thin Solid

Films 2014, 556, 434-439.

83 Moon, D.-Y.; Han, D.-S.; Shin, S.-Y.; Park, J.-W.; Kim, B. M.; Kim, J. H. Thin Solid

Films 2011, 519, 3636-3640.

84 (a) Vidjayacooumar, B.; Emslie, D. J. H.; Clendenning, S. B.; Blackwell, J. M.;

Britten, J. F.; Rheingold, A. Chem. Mater. 2010, 22, 4844-4853, (b) Vidjayacoumar,

B.; Emslie, D. J. H.; Blackwell, J. M.; Clendenning, S. B.; Britten, J. F. Chem.

Mater. 2010, 22, 4854-4866.

Page 49: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

26

85 Lee, B. H.; Hwang, J. K.; Nam, J. W.; Lee, S. U.; Kim, J. T.; Koo, S. –M.;

Baunemann, A.; Fischer, R. A. Sung, M. M. Angew. Chem. Int. Ed. 2009, 48, 4536-

4539.

86 Knisley, T. J.; Ariyasena, T. C.; Sajavaara, T.; Saly, M. J.; Winter, C. H. Chem.

Mater. 2011, 23, 4417-4419.

87 Kalutarage, L. C.; Clendenning, S. B.; Winter, C. H. Chem. Mater. 2014, 26, 3731-

3738.

88 (a) Patterson, G. S.; Holm, R. H. Bioinorganic Chemistry 1975, 4, 257-275, Yokoi,

H.; Addison, A. W. Inorg. Chem. 1977, 16, 1341-1349.

89 (a ) Krisyuk, V. V.; Sysoev, S. V.; Rumyantsev, Y. M.; Prokhorova, S. A.;

Maximovskiy, E. V.; Kosinova, M. L.; Igumenov, I. K. Physics Procedia 2013, 46,

174-182, (b) Krisyuk, V. V.; Baidina, I. A.; Korolkov, I. V.; Semyannikov, P. P.;

Stabnikov, P. A.; Trubin, S. V.; Turgambaeva, A. E. Polyhedra 2013, 49, 1-6, (c)

Rajendran, N. M.; Maheswari, K.; Reddy, D. Polyhedron 2014, 81, 329-334, (d)

Melzer, M. M.; Mossin, S.; Dai, X.; Bartell, A. M.; Kapoor, P.; Meyer, K.; Warren,

T. H. Angew. Chem. Int. Ed. 2010, 49, 904-907.

90 Korolev, A. V.; Lansalot-Matras, C. “Heteroleptic Pyrrolecabaldimine Precursors”

U.S. Patent 8,431,719, Apr. 30, 2013.

Page 50: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

27

Synthesis and Thermal Chemistry of Copper (I) Guanidinates 2 Chapter:

Modified from original manuscript published as:

Coyle, J. P.1; Monillas, W. H.

2; Yap, G. P. A.

2; Barry, S. T.

1 “Synthesis and Thermal

Chemistry of Copper(I) Guanidinates” Inorg. Chem. 2008, 47, 683-689

1 Department of Chemistry, Carleton University, 1125 Colonel By Drive, Ottawa,

Ontario, Canada K1S 5B6. 2 Department of Chemistry and Biochemistry, University of Delaware, Newark,

Delaware 19716.

Abstract 2.1

Copper (I) guanidinate dimers were generated by a salt metathesis route, and

structurally characterised. The guanidinates differed from the known amidinate dimers

because of a large torsion of the dimer ring. This had a direct effect on their thermal

chemistry. Thermal reactivity was investigated by several methods, including a novel

temperature-resolved, gas-phase method that was monitored by mass spectrometry. The

copper guanidinates underwent carbodiimide deinsertion to produce copper metal at

temperatures between 225 – 250 °C in the gas phase, and at 125 °C in solution. The

amidinate investigated also showed copper deposition at 190 °C in the gas phase, and 135

°C in solution, but without carbodiimide deinsertion. The guanidinate compounds

deposited crystalline copper at 225 °C in a simple CVD experiment.

Introduction 2.2

Thin copper films are important to the advancement of microelectronic devices,

and both chemical vapour deposition (CVD)1

and atomic layer deposition (ALD)2 are

methods predicted to be used for copper interconnect production by the International

Technology Roadmap for Semiconductors.3 Organometallic copper precursors have been

Page 51: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

28

studied intensely as vaporous precursors for thin metal film deposition by ALD for this

reason.4 Among copper precursors, copper (I) compounds employing chelate ligands

have shown tremendous utility in both CVD and ALD applications. Examples of these

compounds include copper (I) and (II) β-diketonates,5 as well as copper (I) ketoiminates,

6

and β-diketimidates.7

Recently, copper (I) amidinate dimers have been reported as ALD precursors,8 as

well as to investigate spin delocalization between copper metal centres.9 These species

exist as dimers wherein the amidinate ligand bridges two copper centres. We have

extended this family of copper compounds to include copper(I) guanidinates. The

exocyclic amido moiety will change the bonding mode of the ligand by permitting an

additional resonance structure to exist for the compound (Figure 2.1). When the ligand

has an alkyl in the exocyclic position (Figure 2.1a), the π system is restricted to the dimer

ring. When the exocyclic position is occupied by an amide, the π system can extend to

the exocyclic nitrogen, permitting the “iminium” resonance structure C (Figure 2.1b).

We were interested if this change in resonance, and its concomitant change in bonding

within the dimer ring, would affect the thermal chemistry of the precursor.

Figure 2.1 Resonance Structures for Copper Amidinate and Guanidinate Ligands.

Page 52: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

29

Specifically, our interest in copper guanidinate thermal chemistry is to determine

whether carbodiimide deinsertion plays a role in their decomposition, as has been

demonstrated in aluminum and gallium guanidinates (Figure 2.2).10,11,12

Figure 2.2 Thermally Induced Carbodiimide Deinsertion.

We have synthesized and structurally characterized two copper guanidinates, and

investigated their thermal reactivity through a number of experiments. Most

significantly, we have adapted a quadropole mass spectrometer to sample a thermolysis

apparatus as the precursor vapour is passed through (see Experimental Procedures). By

coupling the time-resolved sampling capacity of the spectrometer with the temperature

ramp of the furnace, we are able to extract a temperature-resolved mass spectrum of

vapour phase species. This experiment allows us to explore the thermal behaviour of the

precursors under the conditions they experience during a typical vapour deposition

experiment. We have also studied the thermolysis of the known amidinate

[MeC(iPrN)2Cu]2,

8d in order to compare thermolysis between amidinates and

guanidinates for copper. Finally, the new guanidinate compounds are shown to deposit

crystalline copper films at 225 °C in a simple CVD experiment.

Results and Discussion 2.3

To determine the role of carbodiimide deinsertion on copper-containing systems,

we have synthesized and studied two copper (I) guanidinates: [Me2NC(iPrN)2Cu]2 (1)

Page 53: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

30

and [iPrN(H)C(

iPrN)2Cu]2 (2). Both of these compounds were made at room

temperature by salt metathesis:

RC(iPrN)2Li + CuCl → 1/2 [RC(

iPrN)2Cu]2 + LiCl,

where R = Me2N (1) and iPrN(H) (2). These compounds formed in excellent yields (96 %

1, 89 % 2), and the simplicity of their 1H NMR spectra suggested a symmetrical structure

in both cases. Single X-ray quality crystals for both 1 and 2 were grown from Et2O, and

their structures were determined (Figure 2.3, Tables 2.1 and Tables 2.2).

Figure 2.3 Single crystal X-ray structures for compounds 1 and 2. Hydrogen atoms were

omitted for clarity, and the thermal ellipses are shown at 30%.

Both compounds have a C2 axis perpendicular to the Cu–Cu axis. The C2 axis in 1

is parallel to the mean plane of the N atoms; in 2 it is perpendicular to the nitrogen atom

plane. The Cu–N bond lengths for both compounds are within the range 1.87 – 1.88 Å,

Page 54: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

31

which agrees well with copper amidinates that have the same dimeric structure.8,9

The

Cu–Cu distances in 1 and 2 were 2.42 and 2.43 Å, respectively. This falls within the

range of general Cu–Cu bonds with bridging ligands, and is much shorter than the Cu–Cu

distance in metallic copper.13

These are intermediate to the reported copper distances in

the amidinate dimers (2.40 Å (ref 8) and 2.46 Å (ref 9)). The C–N–C angles are also

similar (120.0° for 1 and 120.5° for 2, compared to 119.6° (ref 8) for 1 to 120.1° (ref 9)

for 2.

The guanidinate compounds’ structures differ in that the ligand-copper plane is

noticeably twisted, and this can be highlighted by considering the N1–N1A–N3–N3A

torsion angle (32.0° for 1 and 37.5° for 2; Figure 2.4), while previously reported

amidinates are much more planar (2.0° (ref 8) and 0° (ref 9)).

Figure 2.4 The dimer cores of (a) 1 and (b) 2, showing the twists induced by

pyramidalization of the chelating nitrogens. Except for the ligands’ sp2 carbon, all

carbon and hydrogen atoms are omitted for clarity, and the thermal ellipses are shown at

30%.

This core twist can be attributed to the participation of the exocyclic amido

moiety of the guanidinates participating in the π system of the chelate ring, effectively

allowing the amides to be slightly pyramidalized (Figure 2.1, structure C). This is

common for guanidinate ligands.11

Page 55: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

32

Table 2.1 Selected Crystal Data and Structure Refinement Parameters

C18H40Cu2N6 (1) C20H44Cu2N6 (2)

fw 467.64 495.69

T (K) 120 120

λ (Å) 0.71073 0.71073

cryst syst orthorhombic monoclinic

space group C2221 C2/c

a (Å) 11.329 23.939

b (Å) 21.308 5.943

c (Å) 9.923 21.238

α (deg) 90.00 90.00

β (deg) 90.00 122.45

γ (deg) 90.00 90.00

V (Å3) 2395 2550

Z 4 4

ρcalcd (mg/m3) 1.297 1.291

abs coeff (mm-1

) 1.788 1.684

refinement method full-matrix least-squares on F2 full-matrix least-squares on F

2

R indices [I > 2σ(I)]a R1 = 0.0360, wR2 = 0.0860 R1 = 0.0440, wR2 = 0.1068

a R1 = Σ||Fo| - |Fc||/ Σ |Fo| and wR2 = (Σw(|Fo| - |Fc|)

2/ Σw|Fo|

2)

1/2.

Page 56: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

33

Table 2.2 Selected bond lengths and angles for compounds 1 and 2.

1 2

selected bond lengths (Å)

Cu1–N1 1.875(2) Cu1–N1 1.875(2)

Cu1–N3 1.876(2) Cu1–N3 1.871(2)

Cu1–Cu1A 2.4233(10) Cu1–Cu1A 2.4289(11)

N1–C1 1.341(3) N1–C1 1.338(3)

N3–C6 1.334(3) N3–C1 1.345(3)

N2–C1 1.396(5) N2–C1 1.399(3)

N4–C6 1.411(5)

selected bond angles (deg)

N1–Cu1–N3 174.75(10) N1–Cu1–N3 173.71(8)

C7–N3–Cu1 117.14(18) C8–N3–Cu1 121.38(15)

C2–N1–Cu1 118.66(18) C2–N1-–Cu1 117.93(13)

N3–C6–N3A 120.4(3) N1–C1–N3A 120.51(19)

N1–C1–N1A 120.4(3)

sum of angles (deg)

N1 358.2 N1 357.8

N3 357.3 N3 360

N2 360 C1 359.9

N4 360

C1 360

C6 360

torsion angles (deg)

N1–N1A–N3–N3A 32 N1–N3A–N3–N1A 37.5

The guanidinate compounds were studied to determine their thermal chemistry,

and compared to the previously reported [MeC(iPrN)2Cu]2 (3).

8 The thermolysis study

was performed in three stages.

Initially, thermogravimetric analyses (TGA) were collected for each compound to

determine their volatility (Figure 2.5 and Table 2.3). All three compounds showed very

similar volatilization, even though their melting points differed significantly. This is also

reflected in the onset of volatilization of the compounds, which did not follow the

Page 57: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

34

melting point trend. As well, each compound showed very low residual mass (<5 % in all

cases). These experiments suggest that all three precursors would be equally good copper

precursors, and might lead one to assume that their deposition and thermal decomposition

chemistries were similar. However, further thermolysis studies revealed that the thermal

chemistry of the copper guanidinates differed significantly from that of the copper

amidinate.

Table 2.3 Thermal Decomposition Data for 1 - 3.

1 2 3

melting point (°C) 110 79 147

onset of volatilization a (°C) 105 87 102

TGA residual mass (%) 1.8 4.6 2.2

initial copper deposition, NMR tube (°C) 125 125 135

onset of deinsertion, NMR tube (°C) 135 135 --

onset of deinsertion, tube furnace (°C) 225 250 -- a Onset of volatilization is considered to be the point in the TGA where 1% of the mass is

lost.

Figure 2.5 Thermogravimetric analyses of 1 (solid line), 2 (bold line), and 3 (grey line).

0%

20%

40%

60%

80%

100%

25 75 125 175 225 275 325

Mass L

oss (

%)

Temperature(°C)

Page 58: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

35

Each compound was subjected to a sealed tube thermolysis, wherein a sealed,

heavy walled NMR tube was heated in a tube furnace at intervals from room temperature

to a maximum of 235 °C. Periodically, 1H NMR spectra were collected to determine

what, if any, thermolysis products were identifiable. For compounds 1 and 2,

characteristic 1H NMR peaks for diisopropylcarbodiimide (CDI) plus dimethylamine for

1 and isopropylamine for 2 were seen at 135°C, and subsequently increased in intensity at

higher temperatures. Deinsertion of CDI from guanidinate ligands is a prevalent

thermolysis route.11,12

Additional support for this thermolysis route was seen by FTIR

spectroscopy. For both 1 and 2, FT-IR analysis of the solution resulting from the NMR

tube thermolysis showed an absorbance at 2120 cm-1

, which is indicative of the

asymmetric stretch of CDI. Very tellingly, copper metal plated out of solution and

deposited on the walls of the NMR tube in both cases, showing that (in solution, at least)

compounds 1 and 2 are viable precursor for copper metal without requiring a reducing

agent.

The most likely decomposition mechanism for these guanidinates is the

deinsertion of carbodiimide. This deinsertion is followed by decomposition of the

resulting copper (I) amide through deprotonation of the amide by another amide to

produce an imine (Figure 2.6). This reactivity has been seen previously by Saegusa.14

Peaks in the FTIR of the thermolysis solution also support this reaction scheme. The

FTIR showed a peak at 1639 cm-1

for both 1 and 2 that is attributed to the imides

resulting from copper amide deprotonation. The corresponding amines were not seen in

the IR, but we speculate that they evaporated during the IR plate preparation.

Page 59: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

36

Figure 2.6 Thermal Decomposition of Copper Guanidinates.

We were interested to see if CDI deinsertion was occurring in the vapour phase

for the guanidinate compounds, and whether the amidinate species would show any CDI

deinsertion at elevated temperatures. Using a furnace coupled to a quadrapole mass

spectrometer, we able to collect temperature-resolved mass spectra. This experiment is

much more indicative of the environment that the precursors would be subjected to in a

CVD or ALD experiment: the precursors are thermolysed at low concentration in the gas

phase, and exposed to the thermolysis zone for a relatively short period of time. Thus,

we anticipated that the thermolysis chemistry would correlate to the TGA, as well as the

solution thermolysis, but the reaction temperatures would not correspond exactly to the

vapour phase experiments.

For 1, a mass signal for the free guanidine (171 amu) was seen to decrease

significantly at 225 °C, with a corresponding increase in the mass signal for carbodiimide

(126 amu) (Figure 2.7). This trend is also apparent in ionization fragments of the

carbodiimide, notably mass 111 amu (CDI – Me). This suggested that at temperatures

below 225 °C, the whole precursor is surviving to reach the mass spectrometer, and

Page 60: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

37

fragmentation in the mass spectrometer produces the guanidine ion. At 225 °C, CDI

begins to thermally deinsert while the precursor is in the tube furnace, and thus it and its

fragments become prominent in the mass spectrum above this temperature. It should be

noted that the CDI is seen to diminish above about 300 °C, where diisopropyl

carbodiimide itself undergoes thermal decomposition.

Although this temperature was greater than the 125 – 135 °C measured in the

sealed tube thermolysis, this is likely a kinetic effect due to the low residence time of the

precursor in the thermolysis zone during the vapour phase experiment. This is a good

indication that this species could be used for ALD deposition below 225 °C, as thermal

decomposition precludes ALD deposition. Above 225 °C, this species might be used as a

CVD precursor for copper metal without requiring a reducing agent.

Figure 2.7 Temperature-resolved mass spectrum of 1 showing the increase in

carbodiimide and a corresponding decrease in the dimethylamido diisopropyl guanidine.

0.0

2.0

4.0

6.0

8.0

150 175 200 225 250 275 300 325 350

Pre

ssu

re (

mic

roT

orr

)

Temperature (°C)

171

126

Page 61: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

38

For 2, the mass signal for the protonated guanidine cation (186 amu) was seen to

decrease significantly at 200 °C (Figure 2.8). The fragments of this species also echoed

this trend. At the same time, the mass signal for CDI (126 amu) started to ramp in very

slowly at approximately 225 °C. The fragments of this species follow this trend, and

were again most obvious for the mass 111 amu. This again suggested that the whole

precursor is surviving to reach the mass spectrometer until temperatures higher than

225°C, where deinsertion starts to play a significant role, similar to 1. Interestingly, the

amidinate 3 gave very different thermal behaviour, even though its thermal chemistry

occurred at similar temperatures (Figure 2.5 and Table 2.3).

Figure 2.8 Temperature-resolved mass spectrum of 2 showing the increase in

carbodiimide and a corresponding decrease in the protonated triisopropyl guanidine

cation.

The NMR tube thermolysis experiment showed no characteristic isopropyl signals

for CDI in the 1H NMR, even up to 235 °C, the practical limit of this thermolysis

0.0

0.2

0.4

0.6

0.8

1.0

150 175 200 225 250 275 300 325 350

Pre

ssu

re (

mic

roTo

rr)

Temperature (°C)

186

126

Page 62: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

39

experiment. Additionally, there was no evidence of carbodiimide in solution FT-IR.

However, copper metal was seen to deposit on the walls of the NMR tube at 135 °C.

The 1H NMR showed no new signals until 235 °C where peaks corresponding to

the amidine ligand appeared. Further thermolysis experiments in a sealed pressure vessel

at 235 °C allowed the isolation of a small amount of air-sensitive, colourless oil as well

as deposited metallic copper. This oil tested positive for copper using a qualitative flame

test, and a GC-MS of the oil showed a single peak at 143 amu, which corresponds with

the mass of the protonated amidine ligand.

Although unambiguous characterization of this oil was not achieved due to its

extreme reactivity and very low isolated mass, we suspect this might be a paramagnetic

homoleptic copper (II) diisopropyl acetamidinate, liberated through disproportionation of

the copper (I) precursor.

[MeC(iPrN)2Cu]2 → Cu(0) + (MeC(

iPrN)2)2Cu

We suspect further thermolysis of the copper (II) acetamidinate leads to protonated

amidine ligand by an unknown decomposition pathway. Similar reactivity has recently

been reported for copper (I) betadiketiminates15

as well as previously in copper (I)

betadiketonate chemistry.16

This reactivity needs to be further disambiguated, and is a

topic of research in our laboratory.

Compound 3 also showed no evidence of carbodiimide deinsertion in the

temperature-resolved MS, to the maximum temperature of this experiment. The

characteristic parent and fragment mass signals at 126 and 111 remaining undetectably

close to zero throughout the temperature range. However, a mass signal for the parent

guanidine cation peak (143 amu) started to decline at about 190 °C with a corresponding

Page 63: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

40

increase in the mass signal for the fragment “iPr-N=C” (69 amu) (Figure 2.9). This

suggests that the main thermal decomposition pathway for the amidinate is not by CDI

deinsertion, but by destruction of the amidinate itself. Unfortunately, the vapour-phase

thermolysis experiment could not identify the potential copper (II) amidinate from

disproportionation, as the mass of this species is above the limit of the mass spectrometer.

Figure 2.9 The temperature-resolved mass spectrum of 3 showing the increase in the

ligand fragment “C=NiPr” and a corresponding decrease in the protonated acetamidine

cation.

Simple CVD experiments were undertaken to demonstrate the utility of 1 and 2 as

precursors. The depositions were performed in a tube furnace at 225 °C under roughing

pump vacuum (~10-3

Torr). Nitrogen carrier gas was used (20 sccm), and this was pulsed

on and off at 3 second intervals. The pulsing was necessary to promote volatilization of

the copper precursor due to the design of the reactor. Silicon (111) with a native oxide

coating was used as a substrate.

0.0

2.0

4.0

6.0

8.0

10.0

12.0

14.0

150 175 200 225 250 275 300 325 350

Pre

ssu

re (

mic

roTo

rr)

Temperature (°C)

69

143

Page 64: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

41

Both guanidinate precursors produced metallic, copper-coloured films. Scanning

electron micrographs showed the films to be microcrystalline to nanocrystalline, which is

commonly the case with vapour-deposited copper (Figure 2.10).17

X-ray diffraction

identified the films as polycrystalline copper in both cases (Figure 2.11), and energy

dispersive X-ray corroborated this fact. The growth is quite different in each case, with 2

showing much larger crystallite formation, a wide variety of shapes. The film grown by 1

consisted mainly of >100 nm crystallites with a faceted “boulder” appearance, while the

film grown from 2 showed “boulders” up to 500 nm, as well as rods, some as long as 2

μm.

Figure 2.10 Scanning electron micrograph of copper films deposited by (a) 1 and (b) 2.

Page 65: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

42

Figure 2.11 X-ray diffraction spectra of copper deposited in a CVD experiment using (a)

1 and (b) 2 as a precursor.

The mass spectrometer data for each compound supported the decomposition

pathway suggested in Figure 2.6. The mass spectra showed parent peaks for the

guanidinate ligands, as well as for CDI and its fragmentation products. The partial

pressure for CDI was higher then that of the parent guanidinate ligands, which is a sign of

deinsertion occurring before fragmentation in the mass spectrometer. Ideally, deposition

of copper by a CDI deinsertion decomposition pathway would show only CDI as a

significant peak in the in situ QMS data; however, a partial pressure of the guanidinate

ligand was detectable during deposition but this was not surprising considering that the

vaporous precursor is unlikely to be totally consumed by deposition. In the case of 1, a

fragment with a mass of 44 amu was abundant in the mass spectrum, registering as high

30 40 50 60 70 80 90

2q (°)

(111)

(200)

(220) (311)

substrate

a

b

Page 66: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

43

as 2x10-4

Torr, which was a very high partial pressure compared to other mass channels.

This could be attributed to the protonated form of the fragment MeN=CH2, as speculated

in Figure 2.6. Similarly for 2, a fragment with a mass of 58 amu showed a partial

pressure of 2x10-5

Torr and was attributed to the protonated form of the fragment

HN=CMe2 (Figure 2.6). It should be noted that these masses are common fragments of

their respective ligands, and thus we are presently studying this thermal decomposition

pathway more closely to verify our suggested mechanism.

Conclusion 2.4

The copper (I) guanidinate compounds show a similar response to temperature as

the copper (I) amidinate: they deposit copper metal at temperatures just above 100 °C in

a sealed tube experiment. However, the guanidinates do so through a carbodiimide

deinsertion reaction, while the amidinate undergoes a more complicated thermolysis,

potentially involving the disproportionation of copper (I) to produce metallic copper and

copper (II). Temperature-resolved mass spectrometry showed that the thermolysis of

both the amidinate and guanidinates decomposed at higher temperatures in the dilute gas

phase, albeit by mechanisms that were similar to their respective sealed-tube

experiments. We attribute the higher decomposition temperature in the gas-phase

experiment to the short exposure time of the precursor to an elevated temperature. This

better emulates the conditions these species would encounter during a typical ALD

experiment, and thus allows the determination of the temperature limit for these species

as ALD precursors. Finally, both compounds 1 and 2 showed deposition of copper metal

at 225 °C without a secondary gas, demonstrating their utility as CVD precursors for

copper metal films.

Page 67: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

44

Experimental 2.5

General Considerations: All manipulations were carried out in an MBraun

Unilab inert atmosphere drybox. Li(iPrN)2CN(H)

iPr was synthesized following literature

preparation for general guanidinate synthesis.18

Lithium dimethyl amide, diisopropyl

carbodiimide, copper (I) chloride were purchased from Aldrich Chemical Company and

used as received. Hexanes and diethyl ether were purified with respect to oxygen and

water using an MBraun solvent purification system, and stored on activated 4A sieves

until used. Guelph Chemical Laboratories in Guelph, Ontario, Canada, performed

combustion analyses.

[Me2NC(iPrN)2Cu]2 (1): In a 50 mL flask, LiNMe2 ( 0.274 g, 5.10 mmol) was

suspended in 30 mL of hexanes. Diisopropylcarbodiimide (0.668 g, 5.30 mmol) was

diluted in 8 mL of hexanes and added dropwise to the suspension of LiNMe2. The

cloudy, pale yellow suspension cleared to a homogeneous pale yellow solution over 2 h

of stirring. CuCl (0.521 g, 5.10 mmol) was added and the mixture was stirred for 18 h,

after which a cloudy light green solution was filtered to afford a light green solid and a

slightly pale yellow solution. Volatiles were removed under reduced pressure to afford a

crystalline off-white solid (1.14 g, 95.9 % crude yield). The solid was dissolved in a

minimal volume of diethyl ether and was kept at -30 oC overnight. Compound 1 was

collected as clear, colourless crystals (0.86 g, 72 %). mp 109 oC. Anal. Calcd for

C18H40Cu2N6: C, 46.23; H, 8.62; N, 17.97. Found: C, 46.51; H, 9.01; N, 18.22 Mass

spectra m/e (relative abundance): 466 (0.1) M+.

1H NMR (300 MHz, C6D6): δ 3.41 [sept,

4H, NCHiPr], δ 2.54 [s, 12H, N(CH3)2], δ 1.29 [d, 24H NCH(CH3)2].

13C NMR (75 MHz,

C6D6): δ 48.22 [CHCH3], δ 27.59 [CHCH3], δ 40.92 [N(CH3)2, δ 171.58 [(iPrN)2CNMe2].

Page 68: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

45

[iPrN(H)C(

iPrN)2Cu]2 (2): In a 250 mL flask, Li(

iPrN)2CN(H)

iPr (7.727 g, 40.4

mmol) was added to a suspension of CuCl (4.0 g, 40.4 mmol) in 100 mL hexanes. The

solution was stirred for 18 h. It was filtered to afford a pale yellow, clear solution.

Volatiles were removed under reduced pressure to yield compound 2 as off-white

crystalline mass (8.9 g, 89 %). The crude product was recrystallized from 10 ml diethyl

ether to afford clear, colourless crystals, (6.69 g, 67 %) mp 79 oC

Anal. Calcd for

C18H40Cu2N6: C, 48.46; H, 8.95; N, 16.95. Found: C, 48.36; H, 9.17; N, 16.58 Mass

spectra m/e (relative abundance): 494 (0.1) M+ .

1H NMR (300 MHz, C6D6): δ 3.64 [sept,

4H, NCHMe2], δ 3.46 [sept, 2H, HNCHMe2], δ 3.06 [d, 2H HNCHMe2], δ 1.30 [d, 24H

NCH(CH3)2], δ 0.97 [d, 12H HNCH(CH3)2]. 13

C NMR (75 MHz, C6D6): δ 27.67

[NCHCH3], δ 47.49 [NCHCH3], δ 23.55 [HNCH(CH3)2, δ 48.44 [HNCH(CH3)2, δ 171.58

[(iPrN)2CNMe2].

Crystallography: Crystals were selected and mounted on plastic loops with

viscous oil and cooled to the data collection temperature. Diffraction data were collected

on a Bruker-AXS APEX CCD diffractometer. All data-sets were treated with SADABS

absorption corrections. Unit-cell parameters were determined by sampling three different

sections of the Ewald sphere. The systematic absences in the diffraction data were

consistent for Cc and C2/c for 2 and, uniquely, for C2221 for 1. Structural solution in the

centrosymmetric space group option for 2 yielded chemically reasonable and

computationally stable results of refinement. The anomalous dispersion factor refined to

nil in 1 indicating that the true hand of the data was determined. The compound

molecules were located on twofold symmetry. All non-hydrogen atoms were refined with

Page 69: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

46

anisotropic displacement parameters. All hydrogen atoms were treated as idealized

contributions. Structure factors are contained in SHELXTL 6.12 program library.19

Sealed NMR tube thermolysis: NMR samples of 1, 2, and 3 were prepared in

thick-walled NMR tubes using C6D6 as solvent. The tubes were sealed while frozen in

liquid nitrogen and under reduced pressure. The three samples were left overnight in a

furnace at the following temperatures 100, 125, 135, 150, 175, 190, 205, 225 and 235 °C.

After each thermolysis, a 1H NMR was collected

Gas Phase Thermolysis (RGA):A bubbler was charged with the compound of

interest and heated to 5 °C above the compound’s melting point to increase vapour

pressure. This was coupled through a high-vacuum fitting to our homemade ALD

reactor, which was run with all of its valves open and with no carrier gas. The vapour was

carried through a tube furnace that was ramped from 150 °C to 450 °C at 3 °/min. The

resulting gas phase species were sampled by a Microvision Plus 1000e “SmartHead” 300

amu quadropole mass spectrometer, thus allowing a temperature-resolved, gas-phase

thermolysis experiment to be carried out.

References 2.6

1 Dopplet, P. Coord. Chem. Rev. 1998, 1785.

2 (a) Leskela, M.; Ritala, M. Angew. Chem., Int. Ed. 2003, 42, 5548. (b) Ritala, M.;

Leskela, M. In Handbook of Thin Film Materials; Nalwa, H. S., Ed.; Atomic Layer

Deposition, Chapter 2; Academic Press: San Diego, CA, 2001; Vol. 1; p. 103.

3 2005 Edition of the International Technology Roadmap for Semiconductors;

http://www.itrs.net/Links/2005ITRS/Home2005.htm.

4 (a) Kim, J. Y.; Kim, Y.-G.; Stickney, J. L. J. Electrochem. Soc. 2007, 154 , 260. (b)

Park, K.-H.; Bradley, A. Z.; Thompson, J. S.; Marshall, W. J. Inorg. Chem. 2006, 45,

Page 70: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

47

8480. (c) Jezewski C.; Lanford W.A.; Wiegand C.J.; Singh J.P.; Wang P.I.;

Senkevich J.J.; Lu T.M. J. Electrochem. Soc. 2005, 152, 60. (d) Mane A.U.;

Shivashankar, S.A. Mat. Sci. Semicon. Proc. 2004, 7, 343. (e) Niskanen A.; Rahtu

A.; Sajavaara T.; Arstila K.; Ritala M.; Leskela M. J. Electrochem. Soc. 2005, 152,

25.

5 (a) Chen, T. Y.; Omnés, L.; Vaisserman, J.; Doppelt, P. Inorg. Chim. Acta 2004, 357,

1299. (b) Bollmann, D.; Merkel, R.; Klumpp, A. Microelectron. Eng. 1997, 37- 38,

105. (c) Lagalante, A. F.; Hansen, B. N.; Bruno, T. J.; Sievers, R. E. Inorg. Chem.

1995, 34, 5781. (d) Wenzel, T. J.; Williams, E. J.; Haltiwanger, R. C.; Sievers, R. E.

Polyhedron 1985, 4, 369.

6 Lay, E.; Song, Y.-H.; Chiu, Y.-C.; Lin, Y.-M.; Chi, Y.; Carty, A. J. Inorg. Chem.

2005, 44, 7226.

7 Park, K.-H.; Marshall, W. J. J. Am. Chem. Soc. 2005, 127, 9330.

8 (a) Li, Z.W.; Rahtu, A.; Gordon, R.G. J. Electrochem. Soc. 2006, 153, 787. (b) Li,

Z.; Barry, S. T.; Gordon, R. G. Inorg. Chem. 2005, 44, 1728. (c) Lim, B. S.; Rahtu,

A.; Gordon, R. G. Nat. Mater. 2003, 2, 749. (d) Lim, B. S.; Rahtu, A.; Park, J.;

Gordon, R. G. Inorg. Chem. 2003, 42, 7951.

9 Jiang, X.; Bollinger, J. C.; Baik, M.-H.; Lee, D. Chem. Commun. 2005, 1043.

10 Rowley, C. N.; DiLabio, G. A.; Barry , S. T. Inorg. Chem. 2005, 44, 1983.

11 Kenney, A. P.; Yap, G. P. A.; Richeson, D. S.; Barry, S. T. Inorg. Chem. 2005, 44,

2926.

12 Brazeau, A. L.; Wang, Z.; Rowley, C. N.; Barry, S. T. Inorg. Chem. 2006, 45, 2276.

13 Cotton, F. A.; Wilkinson, G; Murillo, C. A; Bochmann, M. Advanced Inorganic

Chemistry; 6th ed.; Wiley-Interscience: New York, 1999, p 861.

14 Tsuda, T.; Wantanabe, K.; Miyata, K.; Yamamoto, H.; Saegusa, T. Inorg. Chem.

1981, 20, 2728.

15 Shimokawa, C.; Tachi, Y.; Nishiwaki, N.; Ariga, M.; Itoh, S. Bull. Chem. Soc. Jpn.

2006, 79, 118.

16 (a) Chen, T.-Y.; Vaissermann, J.; Ruiz, E.; Sénateur, J. P.; Doppelt, P. Chem. Mater.

2001, 13, 3993. (b) Chi, K. M.; Shin, H.-K.; Hampden-Smith, M. J.; Duesler, E. N.

Polyhedron 1991, 19, 2293.

Page 71: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

48

17 Kaloyeros A. E.; Eisenbraun E. Annu. Rev. Mater. Sci. 2000, 30, 363.

18 Foley, S. R.; Yap, G. P. A.; Richeson, D. S. Chem. Commun. 2000, 1515 and

references therein.

19 Sheldrick, G. M. SHELXTL 6.12; Siemens XRD: Madison, WI, 2001.

Page 72: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

49

Gas-Phase Thermolysis of a Guanidinate Precursor of Copper 3 Chapter:

Studied by Matrix Isolation, Time-of-Flight Mass Spectrometry and

Computational Chemistry

Modified from original manuscript published as:

Coyle, J. P.1,2

; Johnson, P. A.1,3

; DiLabio, G. A.3; Barry, S. T.

1; Muller, J.

2 “Gas-Phase

Thermolysis of a Guanidinate Precursor of Copper Studied by Matrix Isolation, Time-of-

Flight Mass Spectrometry, and Computational Chemistry” Inorg. Chem. 2010, 49, 2844-

2850

1 Department of Chemistry, Carleton University, 1125 Colonel By Drive, Ottawa,

Ontario, Canada K1S 5B6. 2 Department of Chemistry, University of Saskatchewan, 110 Science Place, Saskatoon,

Saskatchewan, S7N 5C9. 3 National Institute for Nanotechnology, National Research Council of Canada, 11421

Saskatchewan Drive, Edmonton, Alberta, Canada T6G 2M9

Abstract 3.1

The fragmentation of the copper(I) guanidinate [Me2NC(NiPr)2Cu]2 (1) has been

investigated with time-of-flight mass spectrometry (TOF MS), matrix-isolation FTIR

spectroscopy (MI FTIR spectroscopy) and DFT calculations. Gas-phase thermolyses of 1

were performed in the temperature range of 100 – 800 ºC. TOF MS and MI FTIR gave

consistent results, showing that precursor 1 starts to fragment at oven temperatures above

150 ºC, with a close to complete fragmentation at 260 ºC. Precursor 1 thermally

fragments to Cu(s), H2(g) and the oxidized guanidine Me2NC(=NiPr)(N=CMe2) (3). In

TOF MS experiment 3 was clearly indentified by its molecular ion at 169.2 u. Whereas

H2+ was detected, atomic Cu was not found in gas-phase thermolysis. In addition the

guanidine Me2NC(NiPr)(NHiPr) (2) was detected as a minor component among the

thermolysis products. MI thermolysis experiments with precursor 1 were performed and

species evolving from the thermolysis oven were trapped in solid argon at 20 K. These

species were characterized by FTIR spectroscopy. The most indicative feature of the

Page 73: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

50

resulting spectra from thermolysis above 150 ºC was a set of intense and structured peaks

between 1600 and 1700 cm-1

, an area where precursor 1 does not have any absorbances.

The guanidine 2 was matrix-isolated and a comparison of its FTIR spectrum with the

spectra of the thermolysis of 1 indicated that species 2 was among the thermolysis

products. However, the main IR bands in the range of 1600 and 1700 cm-1

appeared at

1687.9, 1668.9, 1635.1, and 1626.6 cm-1

and were not caused by species 2. The oxidized

guanidine 3 was synthesized for the first time and characterized by 1H NMR and FTIR

spectroscopy. A comparison of an FTIR spectrum of matrix isolated 3 with spectra of the

thermolysis of 1 revealed that the main IR bands in the range of 1600 and 1700 cm-1

a

due to the presence of 3. Based on DFT calculations at the BLYP/6-31G(d) level, the four

bands could be assigned to C=N stretching modes of one isomer of 3. The isomers

exhibit the NMe2 group cis or trans to the iPr group, with cis-3 being significantly less

stable than trans-3. At higher temperature secondary thermal fragments had been

observed. For example at 700 °C, TOF MS and MI FTIR data showed that species 2 and

3, both eliminate HNMe2 to give the carbodiimides iPrNCNiPr (CDI) and

iPrNCN[C(=CH2)Me] (4), respectively. A DFT study of the decomposition of compound

1 was undertaken at the B3LYP/6-31+G(d,p) level of theory employing dispersion-

correcting potentials (DCPs). The DFT study rationalized both carbodiimide deinsertion

and β-hydrogen elimination as exergonic decomposition pathways at 260 °C (G = -44.4

kcal/mol in both cases), but experiment showed β-hydrogen elimination to be the

favourable route.

Page 74: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

51

Introduction 3.2

Thin films of copper metal are of utmost interest in microelectronics, specifically

for use as an interconnect material. Several copper(I) precursors have been reported for

chemical vapour deposition (CVD) and atomic layer deposition (ALD), including -

diketonates,1-4

-diketiminates,5 amidinates,

6-9 and guanidinates

10.

The guanidinate dimer of copper(I), [Me2NC(NiPr)2Cu]2 (1), deposits copper in a

CVD process above 225 °C as a nanocrystalline film;10

similar reactivity is known for the

acetamidinatocopper(I) dimer.9 An interesting aspect of the deposition is that these

precursors act as single source precursors for copper, meaning that they do not require a

second, reducing precursor to produce copper metal. The solution-phase thermolysis of

the guanidinate compound 1 showed the production of diisopropylcarbodiimide (CDI),

and thus we suggested a mechanism whereby CDI deinserted from the ligand to produce

a copper amide intermediate, Cu2(NMe2)2, which then eliminated an imine and an amine

to produce metallic copper (Figure 3.1).10

Figure 3.1 Decomposition of a Copper Guanidinate via CDI Deinsertion

We wanted to further investigate this mechanism, particularly in light of a recent

report of β-hydrogen elimination as a potential thermolysis route.11

In addition, we

recently unraveled the fragmentation of an alumina ALD precursor, the aluminum

guanidinate [Me2NC(NiPr)2]Al(NMe2)2, by time-of-flight mass spectrometry (TOF MS)

and matrix-isolation FTIR spectroscopy (MI FTIR spectroscopy).12

Using these

Page 75: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

52

techniques, we have shown that this precursor eliminates CDI to give the monomeric

aluminum amide Al(NMe2)3 above 300 ºC.12

Thus, we employed these techniques to

further investigate the gas-phase thermolyses of the copper precursor 1 in the temperature

range of 100 – 800 ºC. We report on results of TOF MS, MI FTIR spectroscopy, and

DFT calculations.

Results and Discussion 3.3

Since Pimentel’s pioneering work on matrix-isolation spectroscopy,13,14

this

technique matured into a well-known method to trap and identify reactive intermediates.

Mass spectrometry is a highly sensitive method to investigate gas-phase species and it

has been used to elucidate thermal fragmentations of precursors. Recently, we combined

both techniques in a unique apparatus in which the thermolysis of a CVD precursor can

be investigated using MI FTIR spectroscopy and TOF MS.12

The facility was designed in

such a way that a series of experiments can be performed using one method, which can

then be followed by a similar series of experiments on the same precursor sample and

carrier gas supply using the second method. Consequently, MI FTIR and TOF MS data

are collected consecutively, but the conditions in both series of experiments are kept as

similar as possible so that their data complement one another.

TOF Mass Spectrometry. The mass spectrum at the bottom of Figure 3.2 shows

the typical ion pattern of precursor 1 in the absence of any thermal decomposition; all

fragments of the molecular ion were caused by ion impact ionization at 70 eV of the

precursor 1. An oven temperature of 130 ºC was used to avoid any build-up of 1 in the

apparatus through condensation. The highest detectable masses in this spectrum are due

to M+ of 1 (enlargement in Figure 3.2); its isotopic pattern agrees well with the calculated

Page 76: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

53

one (see Experimental Section). It should be noted that the ion at 465.3 u is not part of the

isotopic pattern of 1+, but results from the loss of one H atom (1

+ - H). When the oven

temperature was increased to 260 ºC (Figure 3.2 top spectrum), 1+ could no longer be

detected15

and the highest mass appeared at 171.2 u followed by a mass of higher

intensity at 169.2 u. The mass of 171.2 u matches with the empirical formula of C9H21N3+

(calc. mass of 171.17 u) and can be interpreted as the cation of the protonated ligand 2

(Figure 3.3). The peak at 169.2 u fits well to C9H19N3+ (calc. mass of 169.16 u) and can

be interpreted as dehydrogenated 2. From the numerous possibilities to assign a structural

formula to the mass of 169.2 u, we assign structure 3 (Figure 3.3) for reasons that will

become apparent in the following discussion.

Figure 3.2 Overview MS of the copper guanidinate 1 with thermolysis oven at 130 ºC

(no thermal fragmentation; bottom spectrum; M+ of 1 enlarged) and at 260 ºC (complete

thermal fragmentation of 1; top spectrum).

Page 77: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

54

Figure 3.3 Protonated and oxidized ligand with calculated masses.

Figure 3.4 Temperature dependence of intensities of selected ions arising from the

thermolysis of 1 [m/z = 466.3 (1+), 171.2 (2

+), 169.2 (3

+), 2.0 (H2

+) u].

Figure 3.4 shows how signal intensities of selected ions changed in the

temperature range of 130 - 200 ºC. The signal intensity of M+ (466.3 u) of the precursor 1

decrease slightly from 160 to 170 ºC, followed by a steeper decrease at temperatures

above 170 ºC. A comparable change of intensities was observed for the signal of 2+

(171.2 u). At the same time, the signal of 3+ (169.2 u) showed a significant increase in

intensity, which indicates that 3+ is an ion of a thermolysis fragment of precursor 1.

Page 78: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

55

In addition to the identification of the peak at 169.2 u, which we assign to the

structural formula 3 (Figure 3.3), there is a significant increase of the signal intensity at

2.0 u, which is due to the presence of H2+. Copper atoms were not detected in the gas

phase; however, after a long series of thermolyses, the thermolysis oven was inspected

and had a copper color at the oven orifice. This is not surprising, as it was shown that 1 is

a precursor for the thermal deposition of Cu.10

Based on these data, we propose that the

thermolysis of precursor 1 can be described as shown in Figure 3.5. We performed DFT

calculations at the B3LYP/6-31+G(d,p) level of theory employing dispersion-correcting

potentials (DCPs), which showed that the production of 3 through -hydrogen

elimination is thermodynamically favorable at 260 °C (G = -44.4 kcal/mol).16

Figure 3.5 Decomposition of a Copper Guanidinate via β-hydride Elimination.

Compound 3 is the formal dehydrogenated product of the protonated ligand 2 and

it is feasible that 2, instead of 3, is the primary thermolysis product of the precursor 1.

Species 2 could further decompose to give the detected species 3. Therefore, an

independent thermolysis series with the protonated ligand 2 as a starting compound was

undertaken. This study revealed that, for temperatures of up to 800 ºC in the presence of a

copper metal surface, species 2 does not eliminate H2 to give 3. In all mass spectra of 2

Page 79: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

56

the signal at 169.2 u appeared only with negligible intensities compared to that at 171.2 u

(2+).

When considering Figure 3.5, it might seem possible for the reaction to proceed

by disproportion of Cu(I) to Cu(II) and Cu(0), giving an undetected (and perhaps unstable

and transient) copper(II) species. This has been suggested for the amidinate depositing

copper on silicon dioxide.17

However, our DFT calculations (at the B3LYP/6-31+G(d,p)

level of theory with DCPs and making the same assumptions as previous) show this to be

unlikely for a gas phase species: it would have a G of 10.9 kcal/mol (compared to -44.4

kcal/mol for -hydrogen elimination from a copper(I) species). As well, the FTIR

spectra throughout the series of thermolysis experiments did not show any peaks that

could not be assigned specifically to the reactants and products of Figure 3.5.

Specifically, the region from 1500 – 1800 cm-1

(where a C=N stretching mode for a

Cu(II) guanidinate species would appear) contained no unassigned peaks. Finally,

similar mechanistic work for surface-bound copper species on a nickel surface resulting

from the thermolysis of a copper amidinate similarly found no experimental evidence for

a copper(II) species.18

The sum of the evidence suggests that we do not see a copper(II)

species in these experiments.

Considering Figure 3.5, it also seems possible that the decomposition might

proceed by a process involving homolytic scission of the Cu-N bonds to produce free

radical intermediates, which may then disproportionate to form 2 and 3. DFT calculations

at the B3LYP/6-31+G(d,p) level of theory with DCPs indicate that this process is

endergonic by 33.6 kcal/mol, and therefore also unlikely. The thermolysis of copper(I)

alkyls has been studied by Whitesides et al.19-21

Their study of n-butylcopper(I)

Page 80: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

57

compounds revealed a β-hydride elimination pathway.19

The decomposition of 1-

propenylcopper(I) was also found not to proceed by a pathway involving free radical

intermediates despite the stability of the vinyl radical.20

However, neophyl(tri-n-

butylphosphine)copper(I) was found to produce the neophyl radical, which is known to

rearrange to an exceptionally stable radical.21

These studies have shown that free radicals

are unlikely intermediates in the thermolysis of copper(I) alkyls unless the free radical

itself is very stable. Copper(I) amides have been found to decompose via β-hydride

elimination and to be more stable than their corresponding alkyls.22

On this basis, it

seems unlikely that a mechanism involving free radical intermediates is involved in the

decomposition of 1.

Alternatively, one might expect the thermolysis reaction as illustrated in Figure

3.5 to be initiated by the decomposition of the dimer 1 to form two copper guanidinate

monomers, which subsequently decompose. Using DFT calculations, we predict that this

pathway is very unlikely at 260 °C, viz. ΔG = 66.7 kcal/mol for the formation of two

copper(I) guanidinate monomers. In addition, there was no evidence of the monomer

[Me2NC(NiPr)2Cu] in the thermolysis series of the dimer 1; the measured intensities of

signals showing fragments with one Cu atom indicated that they were caused by the

impact ionization of 1 alone.

MI FTIR Spectroscopy. The thermal decomposition of precursor 1 was also

investigated with MI FTIR spectroscopy, using similar experimental conditions as for the

TOF MS experiments discussed above. At oven temperatures of up to 150 ºC, IR spectra

did not change, thus indicating that precursor 1 did not decompose (see Supporting

Information, Figure 3.11). At temperatures of 160 ºC, new IR peaks indicated the onset of

Page 81: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

58

the thermolysis. The most indicative feature of the resulting spectrum was a set of intense

and structured peaks between 1600 and 1700 cm-1

, an area where precursor 1 does not

have any absorbances. Spectrum B of Figure 3.6 shows the result of a thermolysis of 1 at

260 ºC. The investigation of 1 by TOF MS revealed that the protonated ligand 2 was a

product in the gas phase. In order to find out if 2 was also present in the matrices, a MI

FTIR spectrum of the synthesized sample of 2 was measured (Figure 3.6, spectrum A).

The comparison of spectrum A with B indicates that 2 was one of the thermolysis

products of 1. Species 2 has its most intense IR band at 1646.0 cm-1

, which appears as a

shoulder of the intense features between 1600 and 1700 cm-1

in spectrum B (see dotted

line in Figure 3.6). The TOF MS experiments clearly indicated that 3 was one of the key

fragments of the thermolysis of the copper precursor 1 (Figure 3.5). Similarly to the

identification of 2 as a thermolysis product, we intended to identify 3 through comparison

with FTIR spectra. To our surprise, species 3 was unknown in the literature, and

consequently needed to be synthesized.

Page 82: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

59

Figure 3.6 Measured IR spectra of copper guanidinate 1 and its thermolysis products (x

axis, 1500 – 1800 cm-1

; y axis, absorbance). Spectrum A: 2 in solid argon (thermolysis

oven at 260 ºC); see Figure 3.13 for a complete IR spectrum. Spectrum B: results of a

thermolysis of complex 1 at 260 ºC; see Figure 3.12 for a complete IR spectrum.

Spectrum C: 3 in solid argon (thermolysis oven at 260 ºC); residual amounts of 2 have

been electronically eliminated; see Figure 3.14 for a complete IR spectrum.

Based on a known method to synthesize imines from secondary amines,23

2 was

oxidized using 2 equiv. of CuBr2 and 2 equiv. of LiOtBu to give species 3. Species 3 was

first characterized by 1H NMR spectroscopy, which showed that in addition to the target

compound 3, small amounts of the starting compound 2 were present. In particular, the

two singlets of equal intensity at 1.43 and 1.72 ppm (in C6D6) clearly revealed the two

inequivalent Me groups of the N=CMe2 moiety of 3 (Figure 3.3). This compound proved

very difficult to isolate from the parent guanidine and tBuOH, all of which have very

similar boiling points, but the IR was captured in matrix isolation, and matched the

Page 83: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

60

calculated vibrational frequencies such that we are satisfied of its formulation (Figure 3.7,

Figure 3.14 in Supporting Information). We are continuing to try to isolate this material

to further our thermolysis studies of this system.

A so-prepared sample was vaporized and trapped in solid argon; spectrum C of

Figure 3.6 shows the resulting IR spectrum. All measured IR bands of 3 (spectrum C) are

present in spectra of the thermolysis of precursor 1 (spectrum B), giving strong evidence

that 3 is a thermolysis product. The structured IR band in the range of 1600 and 1700 cm-

1 with four maxima at 1687.9, 1668.9, 1635.1, and 1626.6 cm

-1 must be caused by C=N

stretching modes. As compound 3 exhibits two C=N bonds, two C=N stretching modes

are expected in the IR range. The fact that the IR absorbance between 1600 and 1700 cm-

1 shows more than two bands, suggests that perhaps different isomers of 3 are present

upon trapping. In order to better understand the structure of the IR band in the C=N

stretching region, DFT calculations at the BLYP/6-31G(d) level of theory were

performed. The lowest energy structure of 3 (Figure 3.7) has a trans orientation of the

Me2N and the iPr group, and was the only isomer that appeared in an appreciable amount

(Figure 3.7). A second isomer with a cis orientation of the MeN2 and the iPr group is

likely to be trapped, as well, in the solid matrix.

The calculated frequencies of the C=N stretches of trans-3 fit very well to the

experimental data: the calculated (BLYP/6-31G(d))24

/experimental frequencies for

(C6=N1) were 1652.9/1668.9 and for (C1=N2) they were 1598.8/1635.1 cm-1

(Figure

3.7). The calculated intensity pattern (ca. 3:1) also fits well to the measured peak ratios:

the two IR bands at lower frequencies are more intense than those at higher frequencies.

However, these assignments are only tentative. For an unambiguous assignment of

Page 84: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

61

experimental IR bands, a complete vibrational analysis of 3 would be necessary. Such an

analysis would necessarily be based on experimental IR data of different isotopomers of

3, which would require extended synthetic work first. However, such an investigation is

beyond the scope of our present work.

Figure 3.7 Possible isomers of 3 and the optimized structure for trans-3 obtained with

B3LYP/6-31+G(d,p)-DCP.

It is interesting that the thermolysis of the copper(I) guanidinate at these

temperatures found no indication of CDI, as was previously found in sealed NMR tube

thermolysis experiments.11

An extensive DFT study of the decomposition of compound 1

was undertaken, and this helps rationalize these two different thermolysis pathways.

These calculations were undertaken at the B3LYP/6-31+G(d,p) level of theory employing

DCPs.

DFT Calculations. The calculated mechanism showed that 1 undergoes a shift of

a nitrogen atom of one of the guanidinate ligands to a 2 bonding arrangement, as well as

a rotation of one of this ligand’s isopropyl groups such that the hydrogen on this group is

oriented toward one copper centre (Figure 3.8, path A). This step is calculated to be

uphill in free energy by 22.5 kcal/mol. The resulting species A1 is the branching point

between β-hydrogen elimination (path B) and CDI elimination (path C).

Page 85: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

62

Figure 3.8 Calculated fragmentation pathways for precursor 1. Free energies relative to

A1 for the reaction steps are shown (values in parentheses are relative to species 1)

As shown in path B of Figure 3.8, compound 3 can be formed through elimination

of the isopropyl methine proton (located in a δ-position) to form a copper hydride (B1),

Page 86: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

63

which is an uphill process by 13.1 kcal/mol (free energy). The hydride B1 eliminates 3 in

a barrierless process. The path from A1 to the products B2 and 3 is endergonic by 10.5

kcal/mol (33.0 kcal/mol from 1).

Instead of undergoing β-hydrogen elimination, A1 can undergo a shift of the μ2-

nitrogen to coordinate one copper atom, with a concurrent rotation about the Cu-N bond

to allow the exocyclic dimethylamido to coordinate to the other copper atom to form

species C1. This step is thermodynamically downhill by 6.4 kcal/mol. Compound C1 can

then eliminate the dimethylamido moiety to give the copper compound C2, which further

reacts to form C3 and free CDI. Energetically, the process from A1 to products C3 and

CDI is exergonic by 0.8 kcal/mol (but endergonic by 21.6 kcal/mol from 1).

These calculations are a good model for the vapour phase decomposition of 1 to

metallic copper. However, the previously reported thermolysis to eliminate carbodiimide

by deinsertion were performed at lower temperatures and in the solution phase.11

These

calculations also show that carbodiimide deinsertion is reasonable as a decomposition

mechanism, as demonstrated by the convincing divergence at species A1.

Fragmentation at higher temperatures. We investigated the fragmentation of the

copper precursor 1 and the protonated ligand 2 at temperatures of up to 800 ºC, and new

fragments appeared in the thermolyses of both 1 and 2. Figure 3.9 shows the results of

two series of thermolysis, spectrum A for 2 and spectrum B for 1. As shown in Figure

3.9, the amount of species 3 (171.2 u), which is a key fragment of the thermolysis of

precursor 1, decreased with increasing temperature, while only two signals, at 124.1 and

45.0 u, showed a significant increase of intensity. The lower mass at 45.0 u fits to Me2NH

(calculated mass of 45.06 u) and the one at higher mass fits to the carbodiimide 4

Page 87: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

64

(calculated mass of 124.10 u, Figure 3.10). These data indicate that the thermolysis

product 3 eliminates Me2NH to give the carbodiimide 4. This interpretation is consistent

with the decomposition of the protonated ligand 2 (Figure 3.9A). The signal for 2+

dropped off, whereas signals at 126.1 and 45.0 u rose with increasing temperatures,

showing that 2 eliminates Me2NH to give the well-known diisopropylcarbodiimide (CDI,

Figure 3.10). As species 2 is also produced in the thermolysis of 1, its signal at 171.2 u

decreased (Figure 3.9). The intensity for the signal of CDI (126.1 u) varies over the

temperature range but does not show a trend, which might be due to its overall low

intensity.

The TOF MS data and their interpretation are consistent with MI FTIR data

obtained from high temperature thermolyses. For example, in the thermolysis of 2 at 700

ºC we unambiguously identified HNMe2 and CDI, trapped in solid argon (Figure 3.15 in

Supporting Information). In the thermolysis of 1, HNMe2 was identified, but the

unknown carbodiimide 4 could not be unambiguously identified, as a required IR

spectrum for comparison is unknown in the literature. However, an intense and structured

IR band with a maximum at 2127.7 cm-1

clearly indicates the presence of a carbodiimide

(Figure 3.16 in Supporting Information). Moreover, an IR band in the typical range of

C=C valence vibrations at 1649.2 cm-1

supports the proposed structure of 4 (see Figure

3.10). Frequency calculations on 4 at the BLYP/6-31G(d) level of theory give a C=C

stretch at 1639.0 cm-1

and a N=C=N asymmetric stretch at 2164.7cm-1

.

Page 88: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

65

Figure 3.9 Temperature dependences of selected ions of the thermolysis at high

temperatures of 1 (spectrum B) and 2 (spectrum A) [m/z = 171.2 (2+), 169.2 (3

+), 126.2

(4+), 124.1 (CDI

+) 45.0 (HNMe2

+) u]. The intensities of masses at 169.2 and 124.1 u

were negligible in spectrum A (counts between 2 and 22 at sweep rates of 8 x 106).

Figure 3.10 Carbodiimides.

Page 89: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

66

Conclusion 3.4

The fragmentation of the dimeric copper(I) precursor [Me2NC(NiPr)2Cu]2 (1)

have been investigated with TOF MS, MI FTIR spectroscopy, and DFT calculations. The

experimental results showed that precursor 1 fragments above oven temperatures of 150

ºC to release the oxidized guanidine Me2NC(=NiPr)(N=CMe2) (3). In addition to 3, the

formation of H2 was detected by TOF MS. The key intermediate 3 was synthesized

independently in this study and through comparison of FTIR spectra of matrix-isolated 3

with those from thermolysis experiment with copper precursor 1, the formation of the

oxidized guanidine 3 as a product of the thermolysis was proven. The structure of the

major IR bands could be rationalized with the help of DFT calculations, which showed

that species 3 exists as a predomination of the trans isomer. These findings can be

explained by assuming a -hydrogen elimination of the ligands in precursor 1 takes place.

DFT calculations indicated that the two decomposition mechanisms result from the same

parent species (A1), which rationalizes the fact that carbodiimide deinsertion is seen at

lower temperatures in the solution phase, but β-hydrogen elimination is favoured in

higher temperature, gas-phase reactions.

When higher temperatures were explored, it became evident that both species 2

and species 3 underwent deinsertion to form free amine and either CDI or 4, respectively.

This important observation indicates that CDI detected at high temperatures can result

from deinsertion from a thermolysis product, and not necessarily from the precursor

itself.

Page 90: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

67

Experimental 3.5

General Remarks. Complex 1 was synthesized via known procedures11

and

purified by sublimation prior to use (1: 70–77 °C, approximately 10-2

– 10-3

mbar).

Compound 2 and was synthesized via known procedures22

and purified via flask-to-flask

condensation at ambient temperatures (approx. 10-2

– 10-3

mbar).

The matrix isolation and the time-of-flight MS apparatus were separate

instruments each equipped with its own thermolysis oven, both identical in construction.

Both instruments used the same carrier gas supply and were in close proximity so that the

heatable container, loaded with the compound of interest, could be moved from one to the

other instrument without exposing the sample to air. Both instruments used the same

thermolysis oven temperature controller. The facility was constructed in this way so that

a series of experiments with one sample batch could be performed using one method, e.g.

MI FTIR spectroscopy, followed by a series of experiments using the other method, e.g.

TOF MS, and still being able to keep the experimental conditions similar in both

consecutive series of experiments.

Each thermolysis oven was equipped with an Al2O3 tube (OD = 4 mm) with two

parallel, inner canals (ID = 1 mm). The overall length of the Al2O3 tube was 35 mm with

the last 10 mm heated with a tungsten wire, coiled around the outside and coated with

ZrO2 cement. One of the inner canals was equipped with a thermocouple (Thermocoax:

NiCrSi/NiSi), while the second canal was used to let a carrier gas / sample mixture pass

through. With this setup, reliable thermolysis temperatures at the inside of the

thermolysis tube could be measured without exposing the thermocouple to the gaseous

sample. A schematic drawing of the thermolysis oven can be found in reference 2423.

Page 91: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

68

A thermolysis series with compound 1 was done in the temperature range between

100 and 800 ºC for both MI FTIR spectroscopy and TOF MS. The thermolysis of

compound 2 was investigated in the temperatures range 200 to 800 ºC for both MI FTIR

spectroscopy and TOF MS.

Matrix-isolation FTIR spectroscopy. The matrix apparatus consisted of a vacuum

line (Varian TV 551 Navigator; Varian DS 402) and a Sumitomo CSW-71 cryogenic

closed cycle system (Sumitomo Heavy Industries. Ltd.) including a Sumitomo RDK-

415D 4K cold head fitted with CsI windows (vacuum shroud design and fabrication by

Janis Research Company, Inc.). The sample was loaded into a heatable container

connected to the thermolysis oven. In a typical experiment, the evacuated container,

loaded with the compound of interest, was kept at constant temperature (1: 86 °C; 2: 0

°C) while a flow of argon (1.25 sccm; Praxair 6.0) was conducted over the sample (mass-

flow controller: MKS Type 1179A). The resulting gaseous mixture was passed through a

thermolysis oven for 30–90 min and deposited onto a CsI window cooled to 20 K. The

distance between the end of the heated oven tube and the CsI window was 54 mm. The

so-prepared matrices were cooled to 4K for FTIR measurements (Bruker Tensor 27

FTIR; 200 to 5000 cm-1

; resolution of 1 cm-1

).

Time-of-flight mass spectrometry (TOF MS). The apparatus consisted of a

custom designed vacuum chamber (designed by Stefan Kaesdorf, Geräte für Forschung

und Industrie; built by Johnsen Ultravac Inc.), equipped with one roughing vacuum pump

(Varian DS 602) and three turbo vacuum pumps, and a reflectron time-of-flight

spectrometer with electron impact ionization (Stefan Kaesdorf, Geräte für Forschung und

Industrie; time resolution under favorable conditions T/T = 10000). For more details

Page 92: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

69

please see reference 12 (Note that the distance between the end of the heated oven tube to

the orifice of the skimmer was shortened from 12 to 8 mm.). In a typical experiment, the

sample container was kept at constant temperature (1: 90–92 °C; 2: 0 °C) while a flow of

argon was conducted over the sample. To get acceptable signal to noise ratios, the

container temperature for 1 needed for the TOF MS measurements was slightly higher

than those for MI FTIR spectroscopy (see above). For all measurements electron impact

of 70 eV and 1 to 20 million sweeps per oven temperature were applied. The signal of the

carrier gas argon at 40 u was reduced in intensity by using a mass filter at 4.35 kV (delay:

3.1000 s; duration: 0.9000 s). This prevented the MCP detector from exceeding its

detection limit. Calibration of flight times was done within every new series of

measurements using Xe as an additional standard. Calibrations were done with the

following masses: 129

Xe+ (128.90478 u),

129Xe

2+ (64.45239 u),

40Ar

+ (39.96230 u) and

H216

O+ (18.01056 u). As the calibration masses did not span the entire range of measured

ions from 1, the experimental masses were usually within the range of ±0.1 u of the

calculated ones.

Calculated masses of selected ions (intensities in parenthesis): 1+ (C18H40Cu2N6

+):

m/z = 466.19 (100.0 %), 467.19 (19.5 %), 467.19 (2.2 %), 468.19 (89.1 %), 468.20 (1.8

%), 469.19 (17.4 %), 469.19 (2.0 %), 470.19 (19.9 %), 470.20 (1.6 %), 471.19 (3.9 %).

DFT Calculations. All calculations were done using the GAUSSIAN 03 program

package.24

The mechanism of thermolysis of 1 was studied with the B327

LYP28

functional and the 6-31+G(d,p) basis set augmented with dispersion correcting potentials

(DCPs).29

DCPs are atom-centered effective core potentials which are employed to better

account for long-range dynamical correlation effects (i.e. dispersion interactions).

Page 93: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

70

Coefficients for DCPs have been optimized30

for a wide variety of functionals and basis

sets and can be implemented into quantum chemical software simply by appending the

input file. All thermodynamic values discussed in the text are calculated free energies at

260º C. To help interpret the IR spectra acquired, molecular vibrations were studied at the

BLYP/6-31G(d) level of theory. The BLYP functional was used rather than B3LYP as it

is known that unscaled frequencies obtained from BLYP are more accurate than those

from B3LYP.31

Page 94: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

71

Supplemental Information 3.6

Figure 3.11 Species 1 in solid argon (oven temperature at 140 ºC; no decomposition; 220

– 4000 cm-1

). Wavenumbers [cm-1

] of the marked IR bands are 2960.4, 2919.2, 2850.9,

2785.3, 1510.1, 1489.7, 1467.0, 1444.0, 1397.0, 1375.7, 1359.2, 1314.2, 1275.3, 1171.9,

1137.2, 1053.0, 783.2, 733.8, 457.4.

Page 95: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

72

Figure 3.12 Results of a thermolysis of complex 1 at 260 ºC (220 – 4000 cm-1

; same IR

spectrum as Figure 3.6B). Wavenumbers [cm-1

] of the marked IR bands are 3012.8,

2972.8, 2939.2, 2904.6, 2874.2, 2839.4, 2794.6, 1687.9, 1668.9, 1635.1, 1626.6, 1488.4,

1452.9, 1435.4, 1372.5, 1337.4, 1261.9, 1246.2, 1190.7, 1167.9, 1144.8, 1079.1, 1056.6,

1003.2, 942.5.

Page 96: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

73

Figure 3.13 Species 2 in solid argon (thermolysis oven at 260 ºC; no decomposition; 220

– 4000 cm-1

; same IR spectrum as Figure 3.6A). The sample of 2 contained residual

amounts of iPrNCNiPr (CDI), which were electronically eliminated from the IR spectrum

of 2. Wavenumbers [cm-1

] of the marked IR bands are 3408.7, 3013.9, 2975.9, 2941.7,

2873.5, 2836.6, 2811.4, 2794.2, 1646.0, 1486.2, 1457.0, 1435.1, 1367.3, 1348.3, 1308.1,

1254.3, 1169.3, 1146.8, 1129.2, 1058.7, 1031.4, 937.3.

Page 97: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

74

Figure 3.14 Species 3 in solid argon (thermolysis oven at 260 ºC; no decomposition; 220

– 4000 cm-1

; same IR spectrum as Figure 3.6C). The sample of 2 contained small

amounts of iPrNCNiPr (CDI), which were electronically eliminated from the spectrum of

3. Wavenumbers [cm-1

] of the marked IR bands are 3012.9, 2973.4, 2939.3, 2874.6,

2839.5, 2794.5, 1687.9, 1668.9, 1634.9, 1626.7, 1488.5, 1452.2, 1436.8, 1372.3, 1337.3,

1261.9, 1246.1, 1190.7, 1167.6, 1144.6, 1079.4, 1003.2, 942.5.

Page 98: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

75

Figure 3.15 Results of a thermolysis of complex 2 at 700 ºC (220 – 4000 cm-1

).

Wavenumbers [cm-1

] of the marked IR bands are (assignments in parentheses) 3306.0,

2985.6 CDI), 2975.0 (HNMe2), 2940.6 (HNMe2), 2874.4 (HNMe2), 2832.3 (HNMe2),

2789.5 (HNMe2), 2123.5 (CDI; the structure of this IR band changes depending on the

way CDI is deposited in matrices; see reference L. C. Ziffle, A. P. Kenney, S. T. Barry

and J. Müller, Polyhedron, 2008, 27, 1832-1840.), 1645.9 (most intense peak of 2),

1457.6 (HNMe2), 1384.5 (CDI), 1368.4 (CDI), 1319.6 (CDI), 1306.7 (CDI), 1167.7

(CDI), 1150.4 (HNMe2), 1119.8 (CDI), 1020.9 (HNMe2), 935.8 (CDI), 908.6, 728.6

(most intense peak of HNMe2), 632.6 (CDI). The assignment of IR bands to HNMe2 is

based on an independently measured IR spectrum of matrix-isolated HNMe2 in argon (B.

Wittig, J. Müller, unpublished results).

Page 99: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

76

Figure 3.16 Results of a thermolysis of complex 1 at 700 ºC (220 – 4000 cm-1

). Small

amounts of 2 and 3 were electronically eliminated from this spectrum. Wavenumbers

[cm-1

] of the marked IR bands are (assignments in parentheses) 2985.4, 2975.2 (HNMe2),

2940.7 (HNMe2), 2874.4 (HNMe2), 2832.3 (HNMe2), 2789.5 (HNMe2), 2127.7, 1649.2,

1483.3 (HNMe2), 1457.3 (HNMe2), 1439.1 (HNMe2), 1386.9, 1369.6, 1337.9, 1323.8,

1230.4, 1169.0, 1150.3 (HNMe2), 1106.0, 1021.0 (HNMe2), 929.1 (HNMe2), 866.6,

728.7 (most intense peak of HNMe2), 626.1. Note: The marked, but unassigned IR bands

could be tentatively assigned to the new carbodiimide 4. However, an unambiguous

characterization of 4 on the basis of the IR data alone is impossible. The IR band at

1649.2 cm-1

could be caused by the C=C stretching mode of 4 (see Figure 3.10). The

assignment of IR bands to HNMe2 is based on an independently measured IR spectrum of

matrix-isolated HNMe2 in argon (B. Wittig, J. Müller, unpublished results).

Page 100: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

77

References 3.7

1 Chen, T. Y.; Omnes, L.; Vaisserman, J.; Doppelt, P. Inorg. Chim. Acta 2004, 357,

1299-1302.

2 Bollmann, D.; Merkel, R.; Klumpp, A. Microelectron. Eng. 1997, 37-8, 105-110.

3 Lagalante, A. F.; Hansen, B. N.; Bruno, T. J.; Sievers, R. E. Inorg. Chem. 1995, 34,

5781-5785.

4 Wenzel, T. J.; Williams, E. J.; Haltiwanger, R. C.; Sievers, R. E. Polyhedron 1985,

4, 369-378.

5 Park, K. H.; Marshall, W. J. J. Am. Chem. Soc. 2005, 127, 9330-9331.

6 Li, Z. W.; Rahtu, A.; Gordon, R. G. J. Electrochem. Soc. 2006, 153, C787-C794.

7 Li, Z. W.; Barry, S. T.; Gordon, R. G. Inorg. Chem. 2005, 44, 1728-1735.

8 Lim, B. S.; Rahtu, A.; Gordon, R. G. Nature Materials 2003, 2, 749-754.

9 Lim, B. S.; Rahtu, A.; Park, J. S.; Gordon, R. G. Inorg. Chem. 2003, 42, 7951-7958.

10 Coyle, J. P.; Monillas, W. H.; Yap, G. P. A.; Barry, S. T. Inorg. Chem. 2008, 47,

683-689.

11 Wu, J. P.; Li, J. Y.; Zhou, C. G.; Lei, X. J.; Gaffney, T.; Norman, J. A. T.; Li, Z.

W.; Gordon, R.; Cheng, H. S. Organometallics 2007, 26, 2803-2805.

12 Ziffle, L. C.; Kenney, A. P.; Barry, S. T.; Müller, J. Polyhedron 2008, 27, 1832-

1840.

13 Whittle, E.; Dows, D. A.; Pimentel, G. C. J. Chem. Phys. 1954, 22, 1943.

14 Norman, I.; Pimentel, G. C. Nature 1954, 174, 508-509.

15 Only traces of 1+ were detectable; intensity of 466.3 u was 25 counts out of 10

million sweeps.

16 This value was calculated using ΔG = -127.3 kcal/mol for the process 2 Cu(g) → 2

Cu(s) calculated from data tabulated in: Lide, D. R. Handbook of Chemistry and

Physics 79th

Edition; CRC Press: Boca Raton, 1998. Using the same level of theory,

ΔG is computed to be -44.4 kcal/mol for the CDI deinsertion process shown in

Figure 3.1.

Page 101: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

78

17 Dai, M.; Kwon, J.; Halls, M. D.; Gordon, R. G.; Chabal, Y. J. Langmuir 2010,

26,3911-3917

18 Ma, Q.; Guo, H.; Gordon, R. G.; Zaera, F. Chem. Mater., 2010, 22, 352–359.

19 Whitesides, G. M.; Stedronsky, E. R.; Casey, C. P.; San Filippo, J. J. Am. Chem.

Soc. 2002, 92, 1426-1427.

20 Whitesides, G. M.; Casey, C. P.; Krieger, J. K. J. Am. Chem. Soc. 2002, 93, 1379-

1389.

21 Whitesides, G. M.; Panek, E. J.; Stedronsky, E. R. J. Am. Chem. Soc. 2002, 94, 232-

239.

22 Tsuda, T.; Watanabe, K.; Miyata, K.; Yamamoto, H.; Saegusa, T. Inorg. Chem.

1981, 20, 2728-2730.

23 Yamaguchi, J.; Takeda, T. Chem. Lett. 1992, 1933-1936.

24 Frisch, M. J.; Trucks, G. W.; Schlegel, H. B.; Scuseria, G. E.; Robb, M. A.;

Cheeseman, J. R.; J. A. Montgomery, J.; Vreven, T.; Kudin, K. N.; Burant, J. C.;

Millam, J. M.; Iyengar, S. S.; Tomasi, J.; Barone, V.; Mennucci, B.; Cossi, M.;

Scalmani, G.; Rega, N.; Petersson, G. A.; Nakatsuji, H.; Hada, M.; Ehara, M.;

Toyota, K.; Fukuda, R.; Hasegawa, J.; Ishida, M.; Nakajima, T.; Honda, Y.; Kitao,

O.; Nakai, H.; Klene, M.; Li, X.; Knox, J. E.; Hratchian, H. P.; Cross, J. B.; Bakken,

V.; Adamo, C.; Jaramillo, J.; Gomperts, R.; Stratmann, R. E.; Yazyev, O.; Austin,

A. J.; Cammi, R.; Pomelli, C.; Ochterski, J. W.; Ayala, P. Y.; Morokuma, K.; Voth,

G. A.; Salvador, P.; Dannenberg, J. J.; Zakrzewski, V. G.; Dapprich, S.; Daniels, A.

D.; Strain, M. C.; Farkas, O.; Malick, D. K.; Rabuck, A. D.; Raghavachari, K.;

Foresman, J. B.; Ortiz, J. V.; Cui, Q.; Baboul, A. G.; Clifford, S.; Cioslowski, J.;

Stefanov, B. B.; Liu, G.; Liashenko, A.; Piskorz, P.; Komaromi, I.; Martin, R. L.;

Fox, D. J.; Keith, T.; Al-Laham, M. A.; Peng, C. Y.; Nanayakkara, A.;

Challacombe, M.; Gill, P. M. W.; Johnson, B.; Chen, W.; Wong, M. W.; Gonzalez,

C.; Pople, J. A. Gaussian 03; Revision D.02 ed.; Gaussian, Inc.: Wallingford CT,

2004.

25 Farrugia, L. J. J. Appl. Crystallogr. 1997, 30, 565.

26 Müller, J.; Wittig, B.; Sternkicker, H.; Bendix, S. J. Phys. IV 2001, 11, 17-22.

27 Becke, A. D. J. Chem. Phys. 1993, 98, 5648-5652.

28 Lee, C.; Yang, W.; Parr, R. G. Phys. Rev. B 1988, 37, 785-789.

29 DiLabio, G. A. Chem. Phys. Lett. 2008, 455, 348-353.

Page 102: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

79

30 Mackie, I. D.; DiLabio, G. A. J. Phys. Chem. A 2008, 112, 10968-10976.

31 Rauhut, G.; Pulay, P. J. Phys. Chem. 1995, 99, 3093-3100.

Page 103: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

80

Copper Iminopyrrolidinates 4 Chapter:

Modified from original manuscripts published as:

Coyle, J. P.1; Kurek, A.

1; Pallister, P. J.

1; Sirianni, E. R.

2; Yap, G. P. A.

2; Barry, S. T.

1

“Preventing thermolysis: precursor design for volatile copper compounds” Chem.

Commun. 2012, 48, 10440-10442.

Coyle, J. P.1; Pallister, P. J.

1; Kurek, A.

1; Sirianni, E. R.

2; Yap, G. P. A.

2; Barry, S. T.

1

“Copper Iminopyrrolidinates: A Study of Thermal and Surface Chemistry” Inorg. Chem.

2013, 52, 910-917

1 Department of Chemistry, Carleton University, 1125 Colonel By Drive, Ottawa,

Ontario, Canada 2 Department of Chemistry & Biochemistry, University of Delaware, Newark, United

States

Abstract 4.1

Several copper(I) iminopyrrolidinates have been evaluated by thermogravimetric

analysis (TGA) and solution based 1H NMR studies to determine their thermal stability

and decomposition mechanisms. Iminopyrrolidinates were used as a ligand for copper(I)

to block previously identified decomposition routes of carbodiimide deinsertion and β-

hydrogen abstraction. The compounds copper(I) isopropyl-iminopyrrolidinate, (1),

copper(I) tertbutyl-iminopyrrolidinate, (2) and copper (I) tert-butyl-imino-2,2-

dimethylpyrrolidinate, (3) were synthesized for this study, and compared to the

previously reported copper(I) guanidinate [Me2NC(iPrN)2Cu]2 (4). Compounds 1 and 2

were found to be volatile yet susceptible to decomposition during TGA. At 165 °C in

C6D6, they had half-lives of 181.7 h and 23.7 h, respectively. The main thermolysis

product of 1 and 2 was their respective protonated iminopyrrolidine ligand. β-hydrogen

abstraction was proposed for the mechanism of thermal decomposition. Copper(I) tert-

butyl-imino-2,2-dimethylpyrrolidinate (3) demonstrated superior thermal stability and

Page 104: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

81

showed negligible decomposition in TGA experiments up to 300 °C as well as no

decomposition in solutions at 165 °C over 3 weeks. Since compound 3 showed no

thermolysis at 165°C, it was further studied by chemisorption on high surface area silica.

It was found to eliminate an isobutene upon chemisoption at 275 °C.

Introduction 4.2

Copper metal remains an interesting topic for chemical vapour deposition (CVD)

and atomic layer deposition (ALD) due to its use in microelectronics, primarily as an

interconnect.1 One class of particularly well-studied precursors are the amidinates, which

originated from the Gordon group in the early 2000s.2 Copper amidinates have utility in

ALD2a

and CVD3 processes between temperatures of 150 – 240°C when using hydrogen

as a reducing agent. Copper(I)-N,N'-di-isopropylacetamidinate has been shown to

undergo CVD deposition as low as 140°C,4 and produces free amidine, acetonitrile,

propene and iminopropane when allowed to thermally decompose in the absence of a

reducing agent.5 These findings have been corroborated in the surface study work of

copper(I) acetamidinates on nickel where - above 130°C - the self-limiting nature of the

monolayer is compromised and continuous uptake of the copper precursor is observed.

Similar ligand fragments were identified in the surface work as in the gas phase work.

We have previously investigated the thermal decomposition of copper(I)

guanidinates, which are similar to amidinates except that the exocyclic group is an amide,

rather than an alkyl.6,7

Using a guanidinate with isopropyl groups on the chelating

nitrogens, we found two distinct thermal decomposition mechanisms (Figure 4.1). In

solution at lower temperatures, the guanidinate deinserted carbodiimide (CDI) and

produced the parent amine of the exocyclic amide group.6 In the gas phase at greater

Page 105: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

82

than 150°C, the methylene carbon of the isopropyl group on the chelating nitrogen loses a

hydrogen and produces an oxidized guanidine. Hydrogen gas is also found as a

thermolysis side product.7

Figure 4.1 Two Thermal Decomposition Pathways For a Copper(I) Guanidiante Species.

Both of these thermal decomposition mechanisms are troubling from the point of

view of developing a copper precursor for ALD. In the first case, the elimination of the

oxidized guanidinate by β-hydrogen abstraction produces a copper hydride, which readily

eliminates dihydrogen or parent guanidine to produce copper metal. This circumscribes

an ALD process in favour of a CVD process. CDI deinsertion also greatly limits the use

of this precursor in thermal processes. The formation of a (transient) copper-amide bond

creates a species that will readily decompose,8 thus also preventing ALD in favour of a

CVD process.

A re-design of the basic amidinate framework is necessary to remove the known

thermal decomposition pathways of this ligand family. Our group has developed and

extensively characterized a novel iminopyrrolidinate ligand family that has evidenced

good thermal stability. Recently, we have reported a family of volatile, stable aluminum

Page 106: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

83

compounds.9 This ligand has a five-membered ring linking one chelate nitrogen to the

“bridgehead” (i.e., quaternary) carbon of the amidinate, thus preventing CDI deinsertion.

Likewise, the ligand has been synthesized to allow control over the number of β -

hydrogens, resulting in a series of three related copper(I) iminopyrrolidinates (Figure

4.2).

Figure 4.2 Series of Amidinate-Type Ligands with Differing Numbers of β-Hydrogens,

Shown As Their Corresponding Copper(I) Compounds

Herein we introduce three novel copper iminopyrrolidinates (copper(I) isopropyl-

iminopyrrolidinate, 1, copper(I) tertbutyl-iminopyrrolidinate, 2 and copper (I) tert-butyl-

imino-2,2-dimethylpyrrolidinate, 3) to complement our previously reported copper (I)

N',N”-diisopropyl-N,N-dimethyl guanidinate (4).6 A thorough exploration of the thermal

chemistry of these four compounds was made to demonstrate how the redesign of this

ligand has influenced thermal behaviour. We have investigated the thermal stability of

Page 107: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

84

this series in the solid phase using a variety of thermal gravimetric methods, as well as in

solution phase using high resolution 1H NMR of sealed tubes that have been treated at

elevated temperatures to study decomposition kinetics. Finally, due to the superior

thermal stability of 3, we have undertaken a study of the nature of the chemisorbed

species produced on silica by 3 as deposited at 275 °C.

Results and Discussion 4.3

The copper compounds 1–3 were simply made by salt metathesis of copper(I)

chloride with the in-situ generated lithium iminopyrrolidinates. These compounds were

isolated as white crystalline materials in moderate to high yields. Similarly, a recent

paper describes trimeric, heteroleptic copper(I) guanidinates isolated from the attempted

synthesis of [Me2NC(NtBu)2Cu]2.

10 We believe the ring of the iminopyrrolidinates

reported herein was necessary to slightly reduce the steric bulk and permit the isolation of

2 and 3 as a dimeric species (see below).

The synthesis of several iminopyrrolidines was described previously and used 2-

pyrrolidone as a starting material. For the synthesis of tert-butyl-imino-2,2-

dimethylpyrrolidine, a different synthetic route was carried out to increase the conversion

yield of 5,5-dimethyl-2-pyrrolidone (Figure 4.3). The decorated 2-pyrrolidone was not

commercially available and the work-up for its synthesis was labour intensive. This

alternative synthetic route is advantageous as it achieves higher yields at lower

temperatures for the substitution of pyrrolidones with bulky amines.

Page 108: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

85

Figure 4.3 The synthetic procedure for producing the tert-butyl-imino-2-

dimethylpyrrolidine ligand.

The 1H NMR of 2 and 3 was simple, suggesting a symmetrical oligomeric

solution structure, similar to known copper guanidinate dimers.6 However, compound 1

showed a more complex 1H NMR. The doublets for the methyls of the isopropyl moiety

in 1 suggested several environments. It is unclear if these multiple environments were

due to an equilibrium of oligomers or from asymmetry in the molecule, but the relative

integrations of these doublets were dependant on the concentration of 1. Serial dilution

of an NMR sample nor heating of the sample to 60°C did not yield a trivial set of peaks

similar to the spectra of 2. Fortunately, 1 could be isolated as X-ray quality crystals.

The structure of 1 shows a tetrameric arrangement in the solid state with an

orthorhombic Ccca space group (Figure 4.4, Table 4.1). There are 16 tetramers in the

unit cell, but only two that are crystallographically distinct. These molecules each have a

core of four copper atoms that lay in a rhombohedral plane, with the rhombus of one

molecule centred perpendicular to a C2 axis (with a minor torsion angle of 1.31°), and the

other parallel to a different C2 axis (with a torsion angle of 0°). The closest Cu-Cu

contact in the unit cell is 2.76Å, which suggests there is no significant Cu-Cu

interactions.11

This is supported by the fact that the N-Cu-N bonds only deviate from

linearity by about 10°, which is likely caused by steric hinderance in the ligands (see

Page 109: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

86

below). Since the connectivity of the molecules in the unit cell is very similar, only one

molecule will be discussed in depth.

Figure 4.4 Structure of 1, shown with the hydrogens removed for clarity. The thermal

ellipsoids are at 30 %.

Page 110: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

87

Table 4.1 Selected bond lengths and angles for 1 - 3.

Compound 1 Compound 2

Selected Bond Length (Å) Selected Bond Length (Å)

Cu1–Cu2 2.756(1) Cu–Cu 2.481(2)

Cu1–Cu1a 2.995 Cu–N1 1.862(2)

Cu1–N1 1.871(5) Cu–N2 1.887(2)

Cu1–N3 1.861(5) N1–C4 1.336(2)

Cu2–N2 1.885(5) N2–C4 1.328(2)

Cu2–N4 1.894(5) Selected Angle Angle (°)

N1–C4 1.311(8) N1–Cu–N2 175.29(6)

N2–C4 1.337(8) N1–C4–N2 122.05(1)

N3–C11 1.311(8) Compound 3

N4–C11 1.331(8) Selected Bond Length (Å)

N1–C1 1.443(9) Cu–Cu 2.4726(5)

N2–C5 1.458(9) Cu–N1 1.867(1)

N3–C8 1.462(8) Cu–N2 1.887(1)

N4–C12 1.487(9) N1–C4 1.330(2)

Selected Angle Angle (°) N2–C4 1.328(2)

Cu2–Cu1–Cu2 114.13(2) Selected Bond Length (Å)

Cu1–Cu2–Cu1 65.86(1) N1–Cu–N2 175.59(6)

N3–Cu1–N1 170.5(1) N1–C4–N2 122.5(1)

N2–Cu2–N4 170.5(1)

N1–C4–N2 123.6(3)

N3–C11–N4 123.1(3)

Interestingly, the two ligands bonded to any specific copper are bonded through

the same type of nitrogen. For example Cu1 is bonded to the ring nitrogens N1 and N3,

where one might expect the ligands to alternate. Additionally, the isopropyl groups of the

ligand are all oriented towards the copper plane. These observations suggest that there is

a fine balance of steric interference across the copper plane allowing a tetramer to form.

Page 111: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

88

This structure type has been seen previously for group 11.12 The Cu-N bonds in this

molecule have an average length of 1.88Å, which is the same as in 2 and 3.

Considering the ligands oriented parallel to each other and on the same side of the

copper plane, it is obvious that more crowding exists here. The ligands bend out slightly

from one another, on average 26.5° from parallel. As well, there is a slight twist of about

6° across each ligand with respect to the line defined by the coppers which bind them.

The metallocycle C-N bonds are all about equivalent in this molecule (1.31Å –

1.34Å), suggesting complete delocalization of the double bond. The ligand's bridging N-

C-N angle is about 123°, which is slightly larger than 2 – 4.6 This is quite understandable

in the case of the tetramer; however, since the ligand is bridging a significantly large Cu-

Cu distance.

The structures of 2 and 3 are more typical of the expected dimeric structures,

considering 4 (Figure 4.5, Table 4.1). Both compounds crystallized in the monoclinic

P21/c space group with two molecules in the unit cell centred on inversion centres, where

both molecules in the unit cell are identical. The Cu-Cu distance are ~2.5Å, which is

significantly closer than in 1. The copper geometry is very close to linear, contorting by

4. 7° and 4.4° to lengthen the Cu-Cu bond for 2 and 3, respectively. The metallocycle

cores are planar with the core N-C bonds all essentially equivalent (1.33Å – 1.34Å),

suggesting that the inherent double bond character is delocalized between these two

bonds. The parallelogram outlined by the four nitrogens of the metallocycle is more

skewed in 2 than 3 (N2A–N1–N2 angles; 95.0° for 2, 93.6° for 3) which is a result of

similar steric bulk provided by the pyrroline and imino groups in 3.

Page 112: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

89

Figure 4.5 Structure of (a) 3 and (b) 4, shown with the hydrogens removed for clarity.

The thermal ellipsoids are at 30 %.

The thermolyses of 1 – 2 were quite encouraging. Compound 1 showed low

residual mass using TGA, and a single feature in weight loss, suggesting that the species

volatilized easily. This low residual mass was surprising. Not only does this compound

possess β-hydrogen atoms for abstraction, but the tetrameric structure was expected to

yield a lower vapour pressure from increased molecular mass. It is possible that there

exists an oligomeric equilibrium that allows 1 to volatilize as a lower order oligomer

(mass spectral analysis shows a dimer), thus providing a larger vapour pressure at lower

temperature. This also explains why 1 has a similar onset of volatilization to the dimeric

compounds 3 and 4.

Compound 2 showed more complex behaviour. The residual mass was 28.1%,

which was close to the percent mass of copper (31.3%) in this compound. The residual

mass was confirmed to be metallic copper by powder X-ray diffraction, suggesting that 2

undergoes a low temperature reduction to produce Cu(0). This has previously been

observed in the case of both 4 and the copper amidinates.4 Due to the presence of the

Page 113: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

90

exocyclic pyrrolidine ring, the more favourable path for this thermal decomposition is β-

hydrogen elimination rather than CDI deinsertion. This can be rationalized considering

the crystal structure of 2. The distortion of the dimer core and lack of steric protection

exposes the copper and enables it to interact with the β-hydrogen atoms of neighbouring

molecules. On the other hand, 3 showed excellent volatile characteristics. Compound 3

has an onset of volatility at 165 °C at atmospheric pressure, with a residual mass of <1%

of the sample mass. It could also be quantitatively sublimed at 130 °C at a pressure of 20

mtorr.

These compounds were also investigated by a thermal stress test using TGA.

Essentially, a compound is measured using the same temperature ramp rate (10 °C/min)

but using different sample masses. Thus, more sample would see higher temperatures

due to the kinetics of thermolysis or volatilization. This valuable test can be used to

gauge the behaviour of the compound with respect to thermal handling during a

deposition process, whether in the source bubbler or during the volatilization and

entrainment to the deposition zone. A good example of this is the thermal stress test of 1

(Figure 4.6b). Compound 1 was shown to have a higher residual mass as the initial pan

loading of the TG was increased. This indicated that it underwent decomposition as more

compound was exposed to higher temperature. Compound 3 (Figure 4.6a) was seen to

undergo no decomposition as pan loading was increased, demonstrating a superior

thermal stability.

Page 114: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

91

Figure 4.6 Thermal stress test of compounds (a) 3 showing no change in residual mass

with increasing sample mass, and (b) 1, showing increasing residual mass with increasing

initial sample mass.

The residual mass trends of each compound 1 – 4 can be seen in Figure 4.7. It

should be noted that the top sample mass that could be accommodated was about 65 mg;

this filled the sample pan in all cases. With the exception of 1, the stress trends are quite

linear with an R2 of 0.99. Compound 1 showed a higher deviation from linearity with an

R2 of 0.97. This might be due to a higher preponderance of a dimeric rather than

tetrameric species at higher temperature, caused by a shift in oligomer equilibrium.

Compounds 1 and 4 show the most stress, deviating from a negligible residual

mass at low loadings to quite high residual masses (13.7 % for 1 and 9.0 % for 4) at high

loadings. It is not surprising that these two compounds show similar thermal stress, since

they both bear an isopropyl group for β-hydrogen elimination although CDI deinsertion

cannot be ruled out in the case of 4.

Page 115: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

92

Figure 4.7 Thermal stress test trends for compounds 1–4. The lines are provided to guide

the eye

Compound 2 again showed poor thermal behaviour with very high residual

masses. Indeed, the highest loading was not attempted for 2 since the 39.5 mg of sample

gave 31.35 % residual mass, which is the mass percent of copper in that compound

(31.32 %). This was not surprising, given the high residual mass seen previously. This

reactivity stands out due to the fact that 2 can be considered of intermediate reactivity

with respect to number of β-hydrogens within this family. However, it has a dimeric

structure (unlike 1, which exists in the solid as a tetramer) and so is less sterically

protected at the copper centres. This would lend it worse thermal stability.

Compound 3 showed very good thermal stress resistance, rising only to 0.56 %

residual mass at 63.0 mg sample mass. This supports our hypothesis that 3 will be the

most thermally stable of this series of compounds due to its lack of reactive hydrogens

and the robust nature of the core of this ligand with respect to CDI deinsertion.

Using TGA, the evaporation kinetics were evaluated for 1 – 4 (Figure 4.8).

Compound 4 showed the highest evaporation at the lowest temperatures. Compounds 1

Page 116: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

93

Figure 4.8 Evaporation kinetics of 1–4 by TGA.

and 2 showed similar evaporation kinetics within the temperatures studied. This is

unsurprising since 1 and 2 are expected to both volatilize as dimers and have similar

molecular masses (a mass difference of only two methyl groups). Surprisingly, 3 showed

the slowest evaporation kinetics even though it has a mass close to that of 4. It is possible

that the measured evaporation kinetics of the copper(I) iminopyrrolidinates are slower

than 4 due to the more rigid framework of the iminopyrrolidinate ligand. The rigidity of

the ligand would cause a compact, planar structure and allow for stronger intermolecular

attraction within the solid. Additionally, the copper(I) iminopyrrolidinates would be

expected to have less entropy gain during volatilization than 4: the rigid ligand has fewer

bonds that are free to rotate in the gas phase than in the solid state, compared to the

relatively less constrained guanidinate of 4. From the isothermal TGA and using the

Langmuir equation,13

the temperatures at which 1 Torr of vapour pressure was obtained

was estimated to be 167°C, 173°C, 204°C, and 138°C for 1 – 4, respectively.14

Page 117: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

94

To further illuminate the thermal chemistry of these compounds, they were each

sealed in heavy walled NMR tubes and heated in an oven at 165°C over a period of days.

An 1H NMR was collected each day to observe their thermal decomposition (Figure 4.9,

Table 4.2). Compound 4 revealed decomposition to produce diisopropylcarbodiimide, as

previously seen.6 The decomposition of 4 that followed first order decomposition kinetics

and had a calculated half-life of 33.8 hours. The parent guanidine was also observed as a

product of thermolysis and its origin of production is discussed below.

Figure 4.9 Thermal decomposition of 1–4 in C6D6 at 165 °C over 21 days.

Compound 1 showed much better thermal behaviour than 4, as was expected from

the TG data. The compound decomposed following first order kinetics with a half-life of

181.1 hours, and there was very obvious plating of copper on the NMR tube walls. The

main byproduct from the thermolysis was the parent ligand, isopropyliminopyrrolidine.

There was no evidence of CDI nor any evidence of oxidized ligand. There was an

Page 118: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

95

obvious flocculant in the NMR tube after the thermolysis; this might be the oxidized

ligand wherein a proton was lost. Compound 2 showed similar decomposition to 1, but

much more quickly (t1/2 = 23.7 hours). The NMR tube was again obscured with plated

Cu(0) and had a flocculant precipitate, and the 1H NMR showed free, protonated ligand.

It is possible that since 1 forms a tetramer, this imparts thermal stability to the compound,

perhaps because the tetramer has to dissociate to a smaller oligomer in order to

thermalise. This would also account for the relatively poor linear fit to first order

kinetics: if the tetramer forms at higher concentration, then there would be a slightly

higher rate of decomposition as the overall concentration of 1 dropped and the dimer-

tetramer equilibrium began to favour the dimer.

Table 4.2 Kinetic data for the thermal decomposition of 1 – 4 at 165°C. The “correlation

coefficient” refers linear fit in Figure 4.9.

Compound Rate Constant

(s-)

Calculated Half‐life

(h)

Correlation Coefficient

1 1.06×10‐6 181.1 0.902

2 8.14×10‐6 23.7 0.944

3 no measurable decomposition

4 5.69×10‐6 33.8 0.995

The full mechanism that produces the protonated ligand remains unclear. We

propose β-hydrogens as the most likely source for protons for the origin of free ligand.

Surface work by Gordon and Zaera4 found that butene elimination occurs from copper(I)-

N,N'-di-secbutylacetamidinate leaving an N-H moiety, which might be another source for

protons. However, no 1H signals were observed in the NMR tube thermolysis experiment

that suggest a similar mechanism occurring here. Evidence for disproportionation of

Cu(I) acetamidinates has also been demonstrated in surface studies on SiO2 substrates.15

Page 119: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

96

Since disproportionation of Cu(I) to Cu(II) and Cu(0) is a common thermolysis route for

Cu(I) compounds, we offer the following insight. We observed a blue colour imparted to

2 during the solution based 1H NMR thermolysis study (Figure 4.9), suggesting the

formation of a Cu(II) species. Attempts to isolate a Cu(II) compound by crystallization

failed and resulted only in the isolation of crystals of 2 with a blue impurity.

Interestingly, we previously had prepared oxidized guanidine (i.e. the product of β-

hydrogen elimination) from the reaction between guanidine and a Cu(II) compound.7

Therefore, a Cu(II) intermediate might be involved in β-hydride abstraction thermolysis

for this class of compound. We are continuing to study the thermolysis mechanisms of

these compounds to gain a fuller understanding of this complicated thermal behaviour.

Compound 3 showed no decomposition at 165 °C over 21 days. It was expected

that its ligand (with no β-hydrogens and without the CDI deinsertion pathway) would

impart the best thermal stability, however this marked difference was surprising. To

further explore this, 3 was subjected to a rigorous surface study. This study used a

combination of solid-state nuclear magnetic resonance (SS-NMR) and high-resolution

NMR (HR-NMR) to determine the initial monolayer and surface chemistry of 3 on high-

surface area silica. SS-NMR has been shown to be a useful tool in analysis of initial

adsorption complexes on high-surface area substrates.16,17

To test compound 1 for vapour phase stability, it was heated in a bubbler at

160°C and the evolved vapour was entrained over high surface area silica for 17 hours

to saturate the silica with a chemisorbed monolayer. Characterization was undertaken

using 1H/

13C cross-polarized magic-angle spinning solid state NMR, and there was

only physisorbed species detected up to 200 °C. At a deposition temperature of 275

Page 120: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

97

°C, solid state 13

C NMR showed signals attributable to the copper precursor (4.10a,

top trace). These signals were similar to the high resolution 13

C NMR of 1 in

deuterated benzene (Figure 4.10a, bottom trace). There was excellent corroboration

between the solution NMR and the solid-state NMR. Although this suggested that the

precursor chemisorbed “whole” at the surface, literature suggests that the alkyl group

at the chelate position might be lost at high temperatures.4 The line width of the

solid-state NMR did not permit unambiguous identification of the tertbutyl moiety, so

another experiment was needed.

The silica with the deposited monolayer was rinsed with D2O to etch off the

surface species, and a high resolution 1H NMR was collected (Figure 4.10b, top

trace), showing a singular surface species. Although the chemical shifts were

different because of the necessity of using different solvents, the integration of the

peaks for the surface species showed loss of the tertbutyl group: integrations of 2.1,

2.0, and 5.7 for the peaks at 2.94 ppm, 2.07 ppm, and 1.36 ppm respectively. The 1H

NMR of the ligand in deuterated chloroform clearly showed a singlet for the tertbutyl

group (4.10b, bottom trace) with integration ratios of 2.0, 2.0, 9.4, and 6.1 for the

peaks at 2.42 ppm, 1.57 ppm, 1.32 ppm, and 1.18 ppm respectively. As well, 29

Si SS-

NMR of the silica showed no additional signals for silicon beyond what was detected

for pure silica, suggesting nucleation did not occur at a silicon atom. This is

reasonable, considering that the most likely nucleation point for this precursor on

silica surface is at the oxygen of a silanol group. Given these data, nucleation likely

occurs through the copper atom to a surface oxygen, and subsequently undergoes

butene elimination (Figure 4.10c). This elimination occurs at 300 °C higher in

Page 121: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

98

temperature than shown for the copper amidinate on metallic surfaces,4 and highlights

the excellent thermal stability designed into this ligand.

Figure 4.10 Reactivity of 1 with silica: (a) shows the SS-13

C NMR of silica after

deposition of 1 at 275°C (top trace) compared to the HR-13

C NMR of 1 in deuterated

benzene (bottom trace). (b) shows the HR-1H NMR of the surface species etched from

the silica with D2O (in D2O; top trace) compared to the HR-1H NMR of 1 in CDCl3

(bottom trace). (c) shows the proposed nucleation and chemisorption of 1 at a silanol

group on a silica surface.

Conclusion 4.4

A series of copper(I) iminopyrrolidinates were synthesized and evaluated by

thermogravimetric analysis and in C6D6 solutions by 1H NMR to determine their thermal

stability and suitability as precursors in CVD processes. The employed asymmetric,

cyclic amidinate ligand proved to impart excellent thermal stability when no β-hydrogens

Page 122: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

99

were present. A direct comparison of the number of β-hydrogens to thermal stability was

complicated by the tetrameric structure of 1, which was thought to influence thermal

stability.

A valuable thermal stress test by TGA was devised and provided complimentary

thermal stability trends to solution based thermolysis studies. Advantages of the thermal

stress test by TGA was faster data collection, and use of conditions more pertinent to

CVD processes. The solution based thermolysis studies identified the parent amidine and

copper metal as thermolysis products of 1 and 2. The amidines were produced through

an intramolecular hydrogen abstraction and a β-hydride abstraction mechanism was

proposed. Compound 3 showed negligible decomposition in both the TGA and solution

experiments, and is an excellent candidate for copper deposition experiments.

Gas-phase experiments suggests that 3 is stable at temperatures >200°C. Surface

analysis suggested that 3 undergoes an alkene elimination from the chelating nitrogen

atom during chemisorption on silica at 275°C.

Experimental 4.5

General Considerations: All manipulations involving the synthesis and handling

of copper(I) compounds were performed in a nitrogen filled drybox. All manipulations

involving the synthesis of the pyrrole and the pyrrolidine were performed in air. The

chemicals CuCl, 2.5 M BuLi in hexanes, tert-butyl amine, and diethyl sulfate were

purchased from Aldrich Chemical Company and used as received. All solvents used in

manipulation of copper(I) compounds were ACS grade and purified from an Mbraun

Solvent Purifier System. All other solvents were ACS grade and used as received.

Nuclear Magnetic Resonance was done on 300 MHz Avance 3 and 400 MHz Bruker

Page 123: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

100

AMX. Canadian Microanalytical Service Ltd. performed combustion analyses. Therm al

gravimetric analysis was performed on a TA Instruments Q50 apparatus located in an

MBraun Labmaster 130 Dry box under a nitrogen atmosphere. 5, 5-dimethyl-2-

pyrrolidone was prepared by literature procedures.18

Tert-butyl ammonium chloride was

prepared by addition of HCl(aq) to tert-butyl amine in ethanol followed by solvent

removal. Isopropyl-iminopyrrolidine and tert-butyl iminopyrrolidine were prepared by

literature procedures.9

Copper(I) isopropyl-iminopyrrolidinate (1): Isopropyl-iminopyrrolidine (5.11 g,

40.49 mmol) was partially dissolved in 60 mL of Et2O and cooled to 0 °C in an ice bath.

16.2 mL of butyl lithium was added dropwise and a suspension formed after stirring for 2

h. In a separate flask, CuCl (4.2 g, 42.42 mmol) was suspended in 60 mL of THF and

cooled to 0 °C in an ice bath. The suspension of lithium isopropyl-iminopyrrolidine was

added via cannula to the cooled suspension of CuCl and was then allowed to warm to

room temperature and stirred overnight. The volatiles were removed from the reaction

flask by reduced pressure and the remaining solid was stirred in 100 mL of toluene for 10

minutes. The cloudy solution was filtered and the clear filtrate was concentrated under

vacuum and kept at -35 °C for 2 days. A mass of small, needle crystals was collected by

filtration, washed with pentane and then dried under vacuum to afford 5.03 g, 65.8%. Mp

138 °C. 1H NMR (400 MHz, C6D6): δ 3.49, δ 3.24 (m, 1H, NCH(CH3)2); δ 3.34, δ 3.26 (

t, 2H, NCH2CH2CH2C); 2.04 (t, 2H, NCH2CH2CH2C); δ 1.58 (quintet, 2H,

NCH2CH2CH2C); δ 1.487, δ 1.304, δ 1.208, δ 1.158 (d, 6H, NCH(CH3)2). 13

C NMR (300

MHz, C6D6) δ 179.84, δ 175.38, δ 54.19, δ 53.30, δ 53.15, δ 51.19, δ 50.48, δ 50.00, δ

29.02, δ 28.69, δ 28.65, δ 27.70, δ 27.55, δ 27.39, δ 27.36, δ 24.99, δ 24.72, δ 24.64.

Page 124: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

101

Combustion analysis, found (calculated): C, 44.63(44.55); H, 7.11(6.94); N,

14.84(14.84).

Copper(I) tertbutyl-iminopyrrolidinate (2): Tert-butyl iminopyrrolidine (1.72 g,

12.26 mmol) was dissolved in 60 mL of THF. 4.9 mL of 2.5 M butyl lithium was added

and the solution was stirred for 2 h. CuCl (1.25 g, 12.62 mmol) was added in one portion

and the suspension was stirred overnight. Volatiles were removed under reduced pressure

and the remaining solid was taken up in THF and filtered. The filtrate was concentrated

and then kept at -35 °C for 1 day. Colourless, block crystals were collected by decanting

the solution, washing with pentane, and then drying under vacuum; obtained 1.59 g, 63.9

%. Mp 148 °C. 1H NMR (300 MHz, C6D6): δ 3.25 (t, 2H, NCH2CH2CH2C), δ 2.19 (t, 2H,

NCH2CH2CH2C), δ 1.63 (quintet, 2H, NCH2CH2CH2C), δ 1.32 (s, 9H, NC(CH3)3). 13

C

NMR (300 MHz, C6D6): δ 180.01 (NCH2CH2CH2C), δ 52.45 (NCH2CH2CH2C), δ 33.72

(NC(CH3)3), δ 33.26 (NC(CH3)3), δ 31.64 (NCH2CH2CH2C), δ 26.33 (NCH2CH2CH2C).

Combustion analysis, found (calculated): C, 47.08(47.39); H, 7.49(7.46); N, 13.69(13.82)

Copper(I) tertbutyl-imino-2,2-dimethylpyrrolidinate (3): Tertbutyl-imino-2,2-

dimethylpyrrolidine (5.103 g, 13.07 mmol) was dissolved in 170 mL of toluene and the

solution was cooled on an ice bath. 12.13 ml of 2.5 M BuLi was added dropwise. The

solution warmed to r.t as it stirred overnight. CuCl (3.26 g, 32.9 mmol) was added and

stirring continued for 18 h. The cloudy, light brown solution was filtered and the filter

cake was extracted with 4 x 20 of THF. Volatiles were stripped from the combined

toluene and THF solutions to afford an off-white solid. The solid was sublimed at 130°C

at 40 mtorr and 5.795 g, 82.7 %, of a white solid was obtained. Mp >270 °C. 1H NMR

(300 MHz, C6D6): δ 2.428 (t, 2H, NC(CH3)2CH2CH2C), δ 1.581 (t, 2H,

Page 125: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

102

NC(CH3)2CH2CH2C), δ 1.328 (s, 9H, NC(CH3)3), δ 1.196 (s, 6H, NC(CH3)2CH2CH2C).

13C NMR (300 MHz, C6D6): δ 177.617 (NC(CH3)2CH2CH2C), δ 61.176 (NC(CH3)3), δ

53.332 (NC(CH3)2CH2CH2C), δ 38.095 (NC(CH3)2CH2CH2C), δ 33.215 (NC(CH3)3), δ

31.931 (NC(CH3)2CH2CH2C), δ 30.940 (NC(CH3)2CH2CH2C). Combustion analysis,

found (calculated): C, 52.44(52.04); H, 8.36(8.30); N, 12.27(12.14).

5-ethoxy-3, 4-dihydro-2,2-dimethyl-2H-pyrrole: Similar to the literature

preparation for 5-ethoxy-3, 4-dihydro-2H-pyrrole:19

5, 5-dimethyl-2-pyrrolidone (9.82 g,

86.8 mmol) and diethyl sulfate (13.38 g, 86.8 mmol) were added to a pressure vessel and

heated for 24 h at 60 °C. Et2O (30 ml) was added and the biphasic mixture was cool in an

ice bath. A 25 ml aqueous solution of Na2CO3 (9.20 g, 86.8 mmol) was added drop wise.

The top organic layer was separated and extraction continued with 3 x 40 ml of Et2O. The

combined extractions were dried over MgSO4. The majority of Et2O was removed on a

roto-vap followed by condensation of the remaining volatiles into a cold trap under

reduced pressure thereby transferring remaining Et2O and product to the cold trap. A

solution of the intended product (11.45 g, 93.4%) in 10.65 g of Et2O was obtained and

used without additional purification. 1H NMR (400 MHz, CDCl3): δ 4.16 (q, 2H,

COCH2CH3), δ 2.53 (t, 2H, NC(CH3)2CH2CH2C), δ 1.80 (t, 2H, NC(CH3)2CH2CH2C), δ

1.30 (t, 3H, COCH2CH3), δ 1.23 (s, 6H, NC(CH3)2CH2CH2C). 13

C NMR (400 MHz,

CDCl3): δ 170.05 (NCO), δ 67.36 (NC(CH3)2), δ 63.67 (OCH2CH3), δ 36.73

(NC(CH3)2CH2CH2C), δ 31.58 (NC(CH3)2CH2CH2C), δ 29.84 (NC(CH3)2CH2CH2C), δ

14.41 (OCH2CH3). HRMS (EI) m/z calcd for C8H15NO M+ 141.1154, found 141.1164.

Tertbutyl-imino-2,2-dimethylpyrrolidine: In a pressure vessel, 5-ethoxy-3,4-

dihydro-2,2-dimethyl-2H-pyrrole (11.45 g, 81.1 mmol) in 10.65 g of Et2O, tert-butyl

Page 126: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

103

ammonium chloride (8.89 g, 81.1 mmol), and tert butyl amine (11.86 g, 162.2 mmol)

were dissolved in 80 mL of ethanol. The pressure vessel was heated to 130 °C for 2 days

with stirring. The vessels was removed from heat and cooled to room temperature.

Volatiles were stripped under reduced pressure. The solid residue was dissolved in 80 mL

of H2O and made basic with 40 mL of 6 M NaOH. The aqueous solution was extracted

with 3 x 60 mL of Et2O. The combined Et2O extractions were dried over Na2SO4 and

then the solution was concentrated under reduced pressure to obtain 11.43 g of a light

yellow liquid, 83.8%. 1H NMR (400 MHz, CDCl3): δ 2.46 (t, 2H, NC(CH3)2CH2CH2C), δ

1.65 (t, 2H, NC(CH3)2CH2CH2C), δ 1.34 (s, (H, NC(CH3)3, δ 1.19 (s, 6H,

NC(CH3)2CH2CH2C) 13

C NMR (400 MHz, CDCl3): δ 161.57 (NCO), δ 69.03

(NC(CH3)2), δ 50.81 (NC(CH3)3), δ 36.60 (NC(CH3)2CH2CH2C), δ 34.62

(NC(CH3)2CH2CH2C), δ 29.85 (NC(CH3)2), δ 29.30 (NC(CH3)3). HRMS (EI) m/z calcd

for C10H20N2 M+ 168.1626, found 168.1618.

Crystallography: X-ray structural analysis for 1 – 3: Crystals were selected and

mounted on plastic mesh using viscous oil flash-cooled to the data collection

temperature. Data were collected on a Bruker-AXS APEX CCD diffractometer with

graphite-monochromated Mo-Kα radiation (λ=0.71073 Å). Unit cell parameters were

obtained from 60 data frames, 0.3º ω, from three different sections of the Ewald sphere.

The systematic absences in the data and the unit cell parameters were uniquely consistent

to Ccca for 1 to P21/c for 2 and 3. The data-sets were treated with SADABS absorption

corrections based on redundant multiscan data.20 The structures were solved using direct

methods and refined with full-matrix, least-squares procedures on F2. The compound

molecules were each located on an inversion point in 2 and 3. Two symmetry unique but

Page 127: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

104

chemically identical molecules of the compound in 1 are each located on a two-fold

rotation axis: in one case the two-fold axis is parallel to the N–Cu–N axis and in the other

case the two-fold axis is perpendicular to the N–Cu–N axis bisecting the Cu atoms on the

opposite distal positions of the tetracopper rhombus. One THF solvent molecule of

crystallization per two tetrameric complexes in 1 was located severely disordered and

treated as diffused contribution.21 One isopropyl group in 1 was located disordered with

a 23/77 refined occupancy ratio. Chemically equivalent bond distances and angles in the

disordered group were restrained to average values with equal atomic displacement

atomic parameter contraints on equivalent atoms. All non-hydrogen atoms were refined

with anisotropic displacement parameters. All hydrogen atoms were treated as idealized

contributions. Atomic scattering factors are contained in the SHELXTL 6.12 program

library.20

Surface Exposure Experiments: The exposure experiments were performed in a

home-built reactor. The reaction chamber consisted of a stainless steel ring support

covered in 200 stainless steel mesh with a plug of glass wool to prevent loss of silica

powder. The system had one inlet from a heated bubbler and one inlet for He (purity of

99.999 %). All fittings used in this system were either CF or VCR to ensure a high-

vacuum seal. The system was leak checked using a gas thermal conductivity/ leak

detector (Gow-Mac Instrument Co.) and an overpressure of He. For the exposure

experiments, typically about 1 g of high surface area SiO2 powder (EP10X; PQ

Corporation; 300 m2/g S.A.; 1.8 cm

3/g P.V.; 24 nm P.S.; 100 μm P.D.) was used. The

powder was pre-treated in the reactor at 350 ˚C for 16 h under vacuum before exposure to

the precursor. The reactor and lines were heated to temperature and allowed to equilibrate

Page 128: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

105

for 1-2 h before introduction of the precursor. The precursor (typically 0.6-0.8 g) was

then vaporized and transported to the substrate with the system under 10-4

Torr vacuum.

The substrate was exposed to volatilized precursor for 17 h before the system was cooled

to room temperature for handling. Both precursor and substrate were handled in inert

atmosphere.

Characterization of Surface Species: Solid-state NMR experiments were

performed at 4.7 T on a Bruker Avance III console. All spectra were obtained using a

Bruker 7 mm 1H/X/Y probe.

13C (ν0 = 50.3 MHz) cross-polarization magic angle

spinning (CP/MAS) experiments were collected at a spinning rate of 4.5 kHz using a 3.4

μs 90° proton pulse with a contact time of 2 ms where the contact pulse was ramped on

the 1H channel. A relaxation delay of 2 s was sufficient to prevent saturation and typically

total acquisition times were 16-30 h. Glycine was used as an external secondary reference

for the 13

C chemical shift scale. Spectra were treated with 40 Hz line broadening during

processing. All spectra were obtained with high power proton decoupling during

acquisition.Samples were prepared for High Resolution NMR (HR-NMR) by adding a

small amount, typically 40-50 mg, of modified silica powder to 2 mL of D2O, agitating,

and allowed to sit for 15 min. The D2O solution was then decanted and studied via HR-

NMR. d4-TSP was used as an internal reference.

References 4.6

1 2011 Edition of the International Technology Roadmap for Semiconductors;

http://www.itrs.net/Links/2011ITRS/Home2011.htm.

2 (a) Li, Z.; Rahtu, A.; Gordon, R. G..J. Electrochem. Soc. 2006, 153, C787, (b) Li, Z.;

Barry, S. T.; Gordon, R. G. Inorg. Chem., 2005, 44, 1728.

Page 129: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

106

3 Krisyuk, V; Aloui, L.; Prud'homme, N.; Sysoev S.; Senocq, F.; Samélor, D.; Vahlas,

C. Electrochem. Solid-State Lett. 2011, 14, D26.

4 (a) Ma, Q.; Guo, H.; Gordon, R. G.; Zaera, F. Chem. Mater. 2010, 22, 352, (b) Ma,

Q.; Guo, H.; Gordon, R. G.; Zaera, F. Chem. Mater. 2011, 23, 3325.

5 Turgambaeva, A.; Prud'homme, N.; Krisyuk, V.; Vahlas, C. J. Nanosci.

Nanotechnol. 2011, 11, 8198.

6 Coyle, J. P.; Monillas, W. H.; Yap, G. P. A.; Barry S. T. Inorg. Chem. 2008, 47, 683.

7 Coyle, J. P.; Johnson, P. A.; DiLabio, G. A.; Barry, S. T.; Muller, J. Inorg. Chem.

2010, 49, 2844.

8 Tsuda, T., Watanabe, K., Miyata, K., Yamamoto, H. and Saegusa, T. Inorg. Chem.

1981, 20, 2728.

9 Wasslen, Y. A.; Kurek, A.; Johnson, P. A.; Pigeon, T. C.; Monillas, W. H.; Yap, G.

P. A.; Barry, S. T. Dalton Trans. 2010, 39, 9046.

10 Willcocks, A. M.; Robinson, T. P.; Roche, C.; Pugh, T.; Richards, S. P.; Kingsley,

A. J.; Lowe, J. P.; Johnson, A. L. Inorg. Chem. 2012, 51, 246.

11 Cotton, F. A.; Daniels, L. M.; Feng, X.; Maloney, D. J.; Matonic, J. H.; Murilio, C.

A. Inorg. Chim. Acta 1997, 256, 291.

12 (a) Abdou, H. E.; Mohamed, A. A.; Fackler, J. P. Jiang, X.; Bollinger, J. J. Cluster

Sci. 2007, 18, 630, (b) Baik, M.-H. Lee, D. Chem. Commun. 2005, 1043, (c) Beck, J.;

Strähle, J. Angew. Chem. Int. Ed. Engl. 1986, 25, 95.

13 Kunte, G. V.; Shivashanker, S. A.; Umarji, A. M. Meas. Sci. Tech. 2008, 19, 025704.

14 The 1 Torr values are corrected from our previous publication (Coyle et al. Inorg.

Chem. 2013, 52, 910) because of a calculation error for the value of the sample pan

surface area.

15 Dai, M.; Kwon, J.; Halls, M. D.; Gordon, R. G.; Chabal, Y. J. Langmuir 2010, 26,

3911.

Page 130: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

107

16 Haukka, S.; Lakomaa, E. L.; Root, A. J. Phys. Chem. 1993, 97, 5085.

17 Wasslen, Y. A.; Tois, E.; Haukka, S.; Kreisel, K. A.; Yap, G. P. A.; Halls, M. D.;

Barry, S. T. Inorg. Chem. 2010, 49, 1976.

18 (a) Moffett, R. B. Organic Synthesis 1952, 32, 59. (b) Osby, J. O.; Ganem, B.

Tetrahedron Lett. 1985, 26, 6413.

19 Beckman, U.; Eichberger, E.; Lindner, M.; Bongartz, M.; Kunz, P. C. Eur. J. Org.

Chem. 2008, 24, 4139.

20 Sheldrick, G.M. Acta Cryst. 2008, A64, 112.

21 Spek, A. L. J. Appl. Cryst. 2003, 36, 7.

Page 131: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

108

Thermally Robust Gold and Silver Iminopyrrolidinates for 5 Chapter:

Chemical Vapour Deposition of Metal Films

Modified from original manuscript published as:

Jason P. Coyle1, Peter G. Gordon

1, Adam P. Wells

1, David J. Mandia

1, Eric R. Sirianni

2,

Glenn P. A. Yap2, Seán T. Barry

1 “Thermally Robust Gold and Silver

Iminopyrrolidinates for Chemical Vapor Deposition of Metal Films” Chem. Mater. 2013,

25, 4566-457

1Department of Chemistry, Carleton University, 1125 Colonel By Drive, Ottawa, K1S

5B6, Canada 2Department of Chemistry & Biochemistry, University of Delaware, Newark, Delaware

19716, United States

Abstract 5.1

Dimeric silver(I) and gold(I) tert-butyl-imino-2,2-dimethylpyrrolidinates were

synthesised and characterised by thermal gravimetric analysis (TGA), differential

scanning calorimetry (DSC), single crystal X-ray diffraction and chemical vapour

deposition (CVD) experiments. The motivation for this work arose from the excellent

thermal stability of the previously reported analogous copper(I) compound and to

complete a series of potential precursors for atomic layer deposition. These compounds

are stable in air and soluble in aromatic or chlorinated solvents. In the solid state, TGA

and DSC showed these compounds to be thermally stable up to 170 °C and to have good

evaporation yields up to 240 °C. Gas phase decomposition temperatures were 140 °C for

the silver compound and 300 °C for the gold compound, as determined by CVD

experiments, where these compounds decomposed to produce metallic films. Reduction

of the metal ions via dehydrogenation of the ligands is proposed as a thermolysis

pathway.

Introduction 5.2

Page 132: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

109

The preparation of metallic films of Cu, Ag, and Au have been a research interest

for several decades. The coinage metals possess the lowest resistivities of all elements

that are suitable for the interconnects in microelectronics. The surface plasmons of these

noble metals1 are well known and they have been employed in photonic devices.

2 Device

fabrication, either for microelectronics or plasmonic devices, routinely employs chemical

vapour deposition3 (CVD) and atomic layer deposition

4 (ALD) for thin film deposition as

they are ideal technologies for coating geometrically complex substrates with high aspect

ratio features in a wide variety of materials.5 The applicability of a CVD or ALD process

relies heavily on its precursor chemistry which often has an important thermal

component.

Precursors for CVD and ALD differ in their surface chemistry. A CVD precursor

is thermally activated by a surface to form the target film either by decomposition or by

reaction with a secondary gas. An ALD precursor is thermally activated to chemisorb to a

surface forming a self-limiting monolayer that is stable throughout the subsequent

purging steps until it reacts with a secondary precursor or reactant. The self-limiting

monolayer consists of a surface species which is often poorly understood yet nevertheless

prevents continuous uptake of gaseous precursor. Careful surface studies by sensitive

techniques are required to fully understand the surface species’ identity.6 The “ALD

window” is a temperature range where the self-limiting monolayer exists and film growth

can occur by reaction with a secondary precursor. This window is observed between the

volatilisation temperature and decomposition temperature of the precursor. Generally, a

precursor is limited for use in CVD when these two temperatures are not adequately

separated.

Page 133: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

110

For copper thin films, the list of precursors for ALD and CVD include many

examples of Cu(I) and Cu(II) homoleptic compounds including β-diketonates,7 β-

diketiminates,8 amidinates,

9 guanidinates,

10 aminoalkoxides

11 and pyrrolylaldiminates.

12

Interestingly, the list of homoleptic precursors for silver and gold is not as populated.

This can be largely attributed to the larger ionic radii of silver and gold compared to

copper. Typically, coinage metal precursors are found in the +1 oxidation state where

copper commonly forms dimeric compounds with the ligands listed above. For silver(I)

and gold(I), non-volatile oligomers or polymers are obtained which require stabilising

Lewis bases to form monomeric or lower-order oligomeric volatile compounds.13

There

exists a larger library of copper precursors due to an industry driven search for the

optimal precursor for the future of interconnects in microchip fabrication.14

Identifying

precursors for silver and gold thin films have generally been an academic pursuit with

potential industrial application. Recently, a previously known CVD precursor for silver

films has been reinvestigated and employed as a plasma enhanced-ALD precursor15

for

the coating of high-aspect ratio substrates for surface-enhanced Raman spectroscopy

(SERS) applications.16

A gold guanidinate17

has been used to coat fibre optics to build

plasmonic devices.18

From the literature, there exist only a few examples of a ligand for which a

complete analogous series of copper, silver, and gold compounds can be prepared for

comparison. For example, homoleptic coinage metal hexamethyldisilazide compounds

form exclusively tetramers.19

These compounds are thermally robust with high melting

points; however, only [CuN(SiMe3)2]4 has been used as a CVD precursor.19a

Coinage

metal N, N’ dialkylamidinates favour dimeric structures with one example of a silver

Page 134: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

111

amidinate existing as a dimer/trimer mixture in solution and the solid state.9d

Copper

amidinates are well-known precursors for ALD9a

but silver and gold amidinates volatilize

and decompose within the same temperature range. Coinage metal alkyl substituted

guanidinates (Figure 5.1) have shown very similar behavior to these alkyl amidinates and

have been used as CVD precursors in homebuilt reactors.10,17

Similarly, coinage metal

carboxylates and perfluorinated carboxylates show a similar trend within this chemical

group20

– generally, the copper compounds are volatile and useful as precursors for CVD

whereas the silver and gold analogues suffer from low thermal stability or low volatility

which impacts their utility as precursors.

Figure 5.1 Amidinates, Guanidinates, and Iminopyrrolidinates Used as Ligands For

Precursors in CVD and ALD (R, R’ = any alkyl group).

Since it is rare for one ligand system to work well across group 11, precursor

design has been developed individually for copper, silver and gold heteroleptic ligand

systems. In addition to the library of homoleptic copper precursors mentioned above,

there are additional entries from monomeric copper(I) compounds stabilised by Lewis

bases. CupraSelect™, (hfac)Cu(TMVS), is a well-known copper precursor for CVD21

-

tethering of the vinyl silane Lewis base to a β-ketoiminate ligand increases thermal

stability.22

Successful silver precursors have been synthesised using oxygen based ligands

(carboxylates, β-diketonates) stabilized by phosphines,13a

alkenes,23

alkynes,24

or

isocyanides.25

Gold precursors can be achieved by ligand systems analogous to silver

precursors26

or by exploiting the stability of methyl Au(I)27

and Au(III)28

compounds. A

Page 135: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

112

variety of Me2Au(III)L compounds have been tested as precursors (where L = β-

diketonates, carboxylates, thiocarbamates, salicylaldiminates, and

dialkyldithiophosphates).

Recently, our group has studied the thermolysis mechanisms of a copper(I)

amidinate29

and a guanidinate30

in the gas phase. These compounds can undergo β-

hydride elimination during decomposition producing metallic films. Redesigning the

amidinate framework to replace β-hydrogen atoms with methyl groups affords an

exceptionally stable, volatile copper compound.31

This redesign also incorporated a five-

membered ring which would prevent carbodiimide deinsertion30,32

and it also lessened the

steric bulk of the ligand to facilitate the formation of a dimer. Herein, we present the

analogous silver(I) and gold(I) compounds and report on their thermal stability,

preliminary results from CVD, and considerations as potential ALD precursors.

Results and Discussion 5.3

Compounds 1 and 2 were generated by salt metathesis of lithium tert-butyl-imino-

2,2-dimethylpyrrolidinate and a metal chloride salt in fair yields (Figure 5.2). The

isolated compounds were air stable and their solubility was limited to benzene, toluene or

methylene chloride. These compounds were insoluble in saturated, aliphatic solvents, and

generally unstable in polar solvents with the exception of methylene chloride. The

isolated yields were lower than other silver and gold amidinates17

and this difference was

attributed to difficulties extracting the product from the crude mixture. The 1H NMR

spectrum of 1 and 2 in C6D6 was simple to interpret and consistent with the expectation

for a single chemical environment. Compound 2 could also be measured in CDCl3 and 1

decomposed immediately in CDCl3.

Page 136: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

113

Figure 5.2 Synthesis of Silver(I) and Gold(I) tert-butyl-imino-2,2-dimethylpyrrolidinate.

Compounds 1 and 2 share an isomorphic dimeric structure with the previously

reported analogous copper compound31

(3) in the monoclinic P21/c space group with two

molecules in the unit cell each located on inversion centres (Figure 5.3, Table 5.1 & 5.2).

The metal-metal distances are 2.677(3) and 2.6801(4) Å for Ag and Au, respectively,

which is similar to previously reported dimeric amidinates.9d,17

In both structures, the

metal ions deviate from the planar metallocycle core bending the N – M – N ideally

linear geometry by ~ 9°. The core C –N bonds range from 1.32 Å – 1.34 Å showing the

expected delocalized bond character within the iminopyrrolidinate. The parallelogram

formed by the four nitrogen atoms in the dimeric molecular core deviates from an ideal

rectangle by 4.9(2)° for 1 and 3.8(2)° for 2 to accommodate for the slight differences in

steric bulk at each end of the asymmetric ligand.

Page 137: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

114

Figure 5.3 Molecular diagram of 2 with thermal ellipsoids at 30% probability. H-atoms

omitted for clarity. Ag analogue compound 1 is isomorphic with 2.

Table 5.1 Crystal Data and Refinement Details of 1 and 2.

1 2

formula C20H38Ag2N4 C20H38Au2N4

crystal system monoclinic monoclinic

space group P21/c P21/c

a (Å) 10.124(10) 10.1692(14)

b (Å) 9.681(9) 9.7129(13)

c (Å) 12.008(12) 12.0353(17)

β (°) 106.047(13) 106.605(2)

V (Å3) 1131.0(19) 1139.2(3)

Z 2 2

ρ (g/cm3) 1.616 2.124

goodness of fit 1.082 1.039

R(Fo) 0.0235 0.0141

wR(Fo) 0.0564 0.0335

Page 138: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

115

Table 5.2 Selected Bond lengths and Angles for 1 and 2

1 2

selected bond length (Å) selected bond length (Å)

Ag - Ag 2.677(3) Au - Au 2.6801(4)

Ag – N1 2.085(2) Au – N1 2.026(2)

Ag – N2 2.102(2) Au – N2 2.047(2)

N1 – C4 1.324(3) N1 – C4 1.337(3)

N2 – C4 1.323(3) N2 – C4 1.333(3)

selected angle angle (deg) selected angle angle (deg)

N1 – Ag – N2 170.43(7) N1 – Au – N2 170.90(9)

N1 – C4 – N2 123.6(2) N1 – C4 – N2 124.7(2)

TGA of 1 and 2 showed single-feature weight loss curves with residual masses

lower than the amount of metal contained in the sample. Equal molar amounts of 1 and 2

were heated under identical conditions and compared (Figure 5.4). The onset of mass loss

(0.5 % weight loss) for 1 was 172 °C and 209 °C for 2. The residual mass from 1 was 13

% which indicates that at least 67 % by mass of the silver in the sample volatilized.

Likewise, the residual mass from 2 was 40 % which indicates at least 26 % by mass of

the gold volatilized. Both compounds decomposed to metal as confirmed by powder X-

ray diffraction (P-XRD).33

Page 139: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

116

Figure 5.4 Thermogravimetric analysis of 1 (black) and 2 (gray). Experiments were run

under 1 atm of nitrogen with a ramp rate of 10 °C/min. Sample sizes for 1 and 2 were

10.49 mg and 13.65 mg, respectively.

Isothermal data for 2 at 210 °C, 230 °C, and 250 °C (Figure 5.5, b) yielded

improved residual masses of 18 % (at least 67% by mass of the gold volatilized). For 1,

isothermal data at 180 °C, 210 °C, and 240 °C yielded residual masses of 7 %, 6%, and

17%, respectively (Figure 5.5, a). The residual mass from 210 °C shows an improved

evaporation yield to 85 % by mass of the silver contained in the sample whereas the

isotherm at 240 °C shows increased decomposition than what was observed at 10 °C/min

(Figure 5.4). Comparison of the isothermal TGA of 1 and 2 highlights 2 as the more

thermally robust compound.

Page 140: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

117

Figure 5.5 . Isothermal TGA of (a) 1 and (b) 2. The furnace was heated at 40 °C/min up

to the isothermal temperature. Isothermal temperatures are indicated in the right hand

legend (°C). Samples sizes were between 3.10 mg to 3.67 mg.

DSC was performed to further evaluate the decomposition temperatures of 1 and

2 and compared to copper(I) tert-butyl-imino-2,2-dimethylpyrrolidinate (3) (Figure 5.6).

DSC traces of 1 showed a broad exothermic peak between 180 – 253 °C; whereas

compound 2 showed a sharper decomposition event at 290 °C. The DSC trace for 3 was

strikingly different and showed endothermic events at 243 °C and 260 °C which were

attributed to melting and boiling points, respectively. For 3, the endothermic events were

repeatable once the sample pan was cooled to room temperature whereas the exothermic

events for 1 and 2 were not repeatable thus indicative of decomposition.

Page 141: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

118

Figure 5.6 Differential scanning calorimetry of 1, 2, and 3 in hermetically sealed

aluminum pans. Temperature ramp was 10 °C/min up to 325 °C. Sample masses were

1.066 mg, 1.625 mg, and 3.790 mg for 1, 2, and 3, respectively. Exotherms are up.

The evaporation kinetics of 1 and 2 were evaluated by stepped isothermal TGA

between 130 °C – 190 °C (Figure 5.7) and compared to 3.34

Both compounds showed

evaporation rates with Arrhenius temperature dependence and the expected trend for

increasing molecular mass. Typically, iminopyrolidinates demonstrate decreased

volatility when compared to acyclic amidinates and guanidinates largely due to their

planar and rigid molecular structure. 34

The design features of iminopyrrolidinates

sufficiently increase thermal stability to allow for higher temperature volatility. From the

stepped isothermal TGA and using the Langmuir equation,35

the temperature at which 1

Torr of vapor pressure could be obtained was estimated to be 222 °C and 238 °C for 1

and 2, respectively.

Page 142: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

119

Figure 5.7 Evaporation kinetics of 1 (♦), 2 (■) and 3 (●).

To further our understanding of the decomposition mechanism, solutions of 1 and

2 in C6D6 were sealed in heavy walled NMR tubes and heated in an isothermal oven

equipped with a light bulb. Compound 2 decomposed at 100 °C whereas 1 required

heating at 120 °C to decompose within the same time frame as 2 (Figure 5.8). Solutions

exposed to light completely decomposed in less time than solutions protected from light.

Both compounds decomposed affording a metallic mirror plated on the NMR tube walls

and protonated ligand as the only observable product by 1H NMR.

Page 143: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

120

Figure 5.8 Decomposition of 1 and 2 in solution (C6D6) measured by 1H NMR.

The mechanism of decomposition remains unclear; however, these results are

consistent with the thermolysis results of previously reported of copper(I)

iminopyrrolidinates.34

Compounds 1 and 2 produced metallic residues during TGA and

solution studies. Since the metal(I) ions were reduced, the ligand must have undergone

sacrificial oxidation. Protonated ligand was the other mechanistic clue which suggests

dehydrogenation of the sacrificial ligand. The calculated yields for protonated ligand in

solution were between 30 – 80 % of the initial concentration which suggests the

unaccounted ligand could have been surface bound in a dehydrogenated state. Similar

chemistry has been proposed for the surface decomposition of copper(I) amidinates,

guanidinates, and iminopyrrolidinates.36

The promising results from thermolyses studies prompted preliminary

investigations of 1 and 2 as precursors for CVD of metallic films. CVD experiments was

Page 144: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

121

carried out in a tube furnace reactor37

on SiO2 and Si substrates. The reactor was slightly

modified and an external container was attached via a KF flange upstream on the tube

furnace to allow for a separate heated zone for the precursor. For 1, the container was

heated up to 110 °C and maintained for 3 h at 35 mtorr. Approximately 50 to 60 mg of 1

Figure 5.9 Film thickness determined from the CVD of 1 (bottom) and 2 (top) at

different furnace temperatures. Depositions with 1 consumed 50 mg - 60 mg of

compound. Depositions from 2 consumed varying amounts: 13.9 mg (300 °C); 21.8 mg

(350 °C); 5.9 mg (400 °C); 20.6 mg (450 °C); 23.5 mg (500 °C).

in an open glass vial was completely volatilized under these conditions for each

deposition. The onset for film deposition was observed at 140 °C which afforded films

less than 5 nm thick. Increasing the substrate temperature in 20 °C increments from 140

Page 145: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

122

to 220 °C afforded increasingly thicker films each with a thickness gradient receding

from the precursor inlet (Figure 5.9, bottom). This series of depositions demonstrates 1 to

be stable in the gas phase and at the substrate surface below 140 °C but is completely

consumed in the tube furnace above temperatures of 200 °C. The deposited films were

confirmed to be metallic silver by P-XRD.33

Images obtained by scanning electron

microscopy (SEM) showed the silver films deposited at 200 °C to be granular with

particle sizes corresponding to film thickness (Figure 5.10; a, b).

Compound 2 was tested in a similar manner as a precursor for CVD of gold films

on Si substrates. Approximately 30 mg of 2 was heated to 130 °C over a 16 h deposition

at 35 mtorr. Upon inspection of the precursor vial it was noticed that the mass of

precursor was not entirely consumed; however, the material remaining consisted of

completely intact precursor as determined by 1H NMR analysis. The onset of film

deposition was found to occur at 300 °C. Increasing the tube furnace temperature in 50

°C increments from 300 °C to 500 °C afforded a thickness profile with a thickness

maximum that migrated towards the precursor inlet at higher temperatures (Figure 5.9,

top). The thickness profile observed for 2 was significantly different than 1 and we

attribute this to a more pronounced temperature gradient across the tube furnace at higher

temperatures. This series of depositions demonstrates 2 to be stable in the gas phase and

at the substrate’s surface below 300 °C. Film thickness at the centre of the tube furnace

reached a maximum at a temperature of 350 °C and deposition occurred predominately at

the precursor inlet at a temperature of 500 °C. The deposited films were confirmed to be

metallic gold by P-XRD.33

Images obtained by SEM of the gold films deposited at 350

°C consisted of densely packed particles that were < 50 nm (Figure 5.10; c, d).

Page 146: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

123

Interestingly, film thickness did not correspond to particle size and the thicker areas

appeared more continuous than granular. The films showed good adhesion by passing a

Scotch tape test.

Figure 5.10 SEM images for thin films deposited from (a, b) 1 and (c, d) 2 at 200 °C and

350 °C, respectively. Images from the CVD of 1 were measured (a) 0.75 cm and (b) 7.75

cm from the precursor inlet. Images from the CVD of 2 were measured (a) 5 cm and (b)

11 cm from the precursor inlet.

X-ray photoelectron spectroscopy (XPS) analysis after sputtering was performed

to determine the bulk composition of the deposited films. The silver and gold films were

of similar purity and contained only carbon as an impurity incorporated from the ligand

system. A film deposited from 1 at 220 °C was determined to be 96.8 at.% silver and 2.7

at.% carbon (Figure 5.12 in Supporting Information) and a film deposited from 2 at 350

°C was determined to be 96.8 at.% gold and 3.2 at.% carbon (Figure 5.13 in Supporting

Page 147: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

124

Information). The remaining composition of these films was oxygen (< 0.5 at.%) which

either arose from exposure to air post-deposition or from background concentrations in

the deposition system. Conductivity measurements of a 156 nm silver film deposited at

220 °C on a glass substrate gave a resistivity of 2.46 μΩ·cm which is close to the value

for bulk silver (1.59 μΩ·cm). Conversely, a 96 nm gold film deposited at 350 °C on a

silicon substrate gave a resistivity of 5.58 mΩ·cm which is significantly higher than bulk

gold (2.44 μΩ·cm). The higher resistivity compared to bulk gold are probably not due to

impurities but rather to poorly connected particles in the film.

In light of the film thickness gradient inherent to the crude reactor design, CVD

experiments using a low flow of N2 gas were performed which successfully minimized

thickness gradients across 20 cm of the furnace by increasing the rate of mass transport of

1 (Figure 5.11). The tube supplying N2 was heated prior to leaking N2 into the vacuum

system behind the precursor. Negligible gradients were observed between 250 °C and

300 °C; above 300 °C the rate of decomposition surpassed the rate of mass transport and

a gradient was observed again. CVD with 1 under N2 flow required higher substrate

temperatures either because the gas flow cooled the surfaces or because mass transport of

the precursor drastically improved. Growth rates calculated from the data in Figure 5.11

gave values between 0.8 nm/min and 1.1 nm/min across 17 cm of the tube furnace (R2

values of the linear fits for growth rate at each distance were between 0.87 – 0.98). A

flow of N2 did not affect the film gradients or temperatures for CVD with 2.

Page 148: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

125

Figure 5.11 Film thickness determined from timed CVD experiments of 1 under a low

flow of N2 at 300 °C with a system pressure of 100 mtorr.

These new compounds are significantly different than the commonly used

precursors for the CVD of silver and gold mentioned above. The formulation of 1 and 2

as N-bonded, homoleptic dimers that are volatile and thermally robust is quite rare for

silver and gold precursors. In consideration of volatility, 1 and 2 are less volatile than

existing precursors; however, they do not require a fluorinated ligand or a Lewis base.

These helpful strategies to increase volatility can lead to film impurities and precursor

decomposition via dissociation of the Lewis base. Compound 1 deposits films at lower

temperatures compared to previously reported precursors, which typically have minimum

deposition temperatures > 200 °C. On the other hand, 2 was found to require higher

substrate temperatures than any previously reported gold precursor – a promising result

for a potential ALD precursor.

Page 149: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

126

Conclusion 5.4

Two thermally robust CVD precursors for silver and gold thin films were

synthesised and thermally characterized. Despite a lack of suitable solvents, the synthetic

yields were satisfactory for our studies. Compounds 1 and 2 are thermally stable up to

170 °C as pure solids. Under low pressure CVD conditions, 1 and 2 could be volatilized

without decomposition between 110 °C – 130 °C. Furthermore, these precursors

remained predominately volatile up to 240 °C during atmospheric TGA.

TGA, DSC and CVD experiments determined 2 to be more thermally stable than

1. The series of coinage metal precursors had the following trend in thermal stability Cu

> Au > Ag in the solid or gaseous state. Solution based thermal studies revealed metallic

mirrors and protonated ligand as the observable decomposition products. The order of

thermal stability for 1 and 2 was reversed in C6D6 solutions and both compounds

demonstrated enhanced decomposition when exposed to light.

Compounds 1 and 2 are improved precursors for CVD applications when

compared to other amidinate and guanidinate compounds – their evaporation temperature

and gas phase decomposition temperatures are well separated which is desirable for CVD

and ALD. The employed ligand design was intended to block low temperature

decomposition pathways of β-hydrogen abstraction and CDI de-insertion.30

Despite this

attempt, 1 and 2 could still be thermally decomposed affording metallic residues and thin

metal films - presumably by dehydrogenation of the ligand at higher temperatures.

Metallic thin films of silver and gold consisting of nanoparticles were deposited between

140 °C – 220 °C and 300 °C – 500 °C, respectively. Low film resistivities for silver films

were achieved while the gold films gave resistivity values two orders of magnitude

Page 150: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

127

higher than bulk gold. This striking difference was likely due to differences in film

morphology. Current investigations are focusing on optimizing CVD conditions and

exploring reducing agents for ALD processes.

Experimental 5.5

General Considerations: Some manipulations (loading, filtering, and isolation)

were performed in an MBraun Labmaster™ 130 Dry box (mBraun, Stratham, NH,

U.S.A.) under a nitrogen atmosphere while additions were performed by standard

Schlenk techniques. NMR spectra were recorded on a 400 MHz Bruker AMX

spectrometer. NMR spectra were measured in C6D6 or CDCl3 and were referenced against

residual protonated solvent or TMS, respectively. Tert-butyl-imino-2,2-

dimethylpyrrolidine31

and THT·AuCl38

were prepared according to literature. AgCl was

purchased from Strem Chemicals and used as received. Toluene and diethyl ether were

purchased as ACS grade and purified from an Mbraun Solvent Purifier System.

Dichloromethane and pentane were purchased as anhydrous from Sigma Aldrich

Chemical Company and used as received. Canadian Microanalytical Service Ltd.

performed combustion analysis. Thermal gravimetric analysis was performed on a TA

Instruments Q50 apparatus located in an MBraun Labmaster 130 Dry box under a

nitrogen atmosphere. Differential scanning calorimetry was performed on a DSC

Instruments Q10 apparatus.

Silver(I) tert-butyl-imino-2,2-dimethylpyrrolidinate (1): Tert-butyl-imino-2,2-

dimethylpyrrolidine (3.364 g, 20.0 mmol) was dissolved in 60 mL of toluene and cooled

to 0 °C. Butyl lithium in hexanes (2.5 M, 8.0 mL, 20 mmol) was added dropwise and the

solution was stirred for 3 h at room temperature. In a separate 500 mL Schlenk flask

Page 151: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

128

wrapped in aluminum foil, AgCl (2.865 g, 20.0 mmol) was suspended in 200 mL of

toluene. The lithiated imino-pyrrolidinate solution was added dropwise via cannula over

1 h and the resulting mixture was stirred for 16 h. The reaction mixture was filtered and

the insoluble solids were washed with 20 mL of toluene. Volatiles were vacuum distilled

from the combined washings and filtrate to afford a light brown solid. The insoluble

solids were washed further with dichloromethane (3 x 20 mL). These washings were

combined and the volatiles were vacuum distilled to afford more of the light brown solid.

The two portions of solid were combined and washed with pentane (4 x 10 mL). The

crude solid was recrystallized from 20 mL of hot toluene in a pressure vessel to afford

colourless, block crystals; 3.615g, 65.7%. 1H NMR (400 MHz, C6D6): δ 1.16 (s, 6H,

NC(CH3)2CH2CH2C), δ 1.29 (s, 9H, NC(CH3)3, δ 1.65 (t, 2H, NC(CH3)2CH2CH2C), δ

2.54 (t, 2H, NC(CH3)2CH2CH2C) 13

C NMR (400 MHz, C6D6): 32.9

(NC(CH3)2CH2CH2C), 33.8 (NC(CH3)2CH2CH2C), 34.0 (NC(CH3)3), 38.3

(NC(CH3)2CH2CH2C), 52.8 (NC(CH3)2CH2CH2C), 61.3 (NC(CH3)3), 175.1 (NCN).

Combustion analysis, found(calculated): C, 43.21(43.65); H, 7.04(6.96); N, 10.15(10.18).

Gold(I) tert-butyl-imino-2,2-dimethylpyrrolidinate (2): Tert-butyl-imino-2,2-

dimethylpyrrolidine (2.874 g, 17.1 mmol) was dissolved in 60 mL of toluene and cooled

to 0 °C. Butyl lithium in hexanes (2.5 M, 6.83 mL, 17 mmol) was added dropwise and

the solution was stirred for 3 h at room temperature. In a separate 500 mL Schlenk flask

wrapped in aluminum foil, THT·AuCl (5.475 g, 17.1 mmol) was suspended in 175 mL of

toluene and cooled to -78 °C. The lithiated imino-pyrrolidinate solution was added

dropwise via cannula over 1 h and the resulting mixture was stirred for 16 h while

gradually warming to room temperature. Volatiles were vacuum distilled to afford a dark

Page 152: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

129

solid which was dried under high-vac to remove residual THT. The solid was stirred with

warm toluene (4 x 50 mL) for 15 min and filtered. The extractions were combined and

volatiles were vacuum distilled to afford a solid that was washed with diethyl ether (4 x

5mL). The solid was dissolved in 20 mL of hot toluene in a pressure vessel and left to

stand for 12 h cooling to room temperature. A crop of colourless, block crystals were

isolated by decanting the supernatant, washing with diethyl ether (3 x 5 mL) and dried

under vacuum to afford 2.100 g. A second crop of product was obtained from the

insoluble solid that remained post toluene extraction. The remaining insoluble solids were

stirred with dichloromethane (4 x 50 mL) for 15 min and filtered. The extractions were

combined and volatiles were vacuum distilled to afford a solid that was washed with

diethyl ether (4 x 5 mL). The solid was dissolved in 20 mL of hot toluene in a pressure

vessel and left to stand for 12 h cooling to room temperature. A second crop of

colourless, block crystals were isolated by decanting the supernatant, washing with

diethyl ether (3 x 5 mL) and drying under vacuum to afford 1.960 g; total yield was 4.060

g, 65.3%. 1H NMR (400 MHz, CDCl3): δ 1.18 (s, 6H, NC(CH3)2CH2CH2C), δ 1.38 (s,

9H, NC(CH3)3), δ 1.72 (t, 2H, NC(CH3)2CH2CH2C), δ 2.73 (t, 2H, NC(CH3)2CH2CH2C)

13C NMR (400 MHz, CDCl3): δ 30.5 (NC(CH3)2CH2CH2C), δ 33.7 (NC(CH3)3), δ 34.2

(NC(CH3)2CH2CH2C), δ 36.8 (NC(CH3)2CH2CH2C), δ 56.0 (NC(CH3)2CH2CH2C), δ

63.4 (NC(CH3)3), δ 176.5 (NCN) Combustion analysis, found(calculated): C,

32.85(32.98); H, 5.23(5.26); N, 7.67(7.69).

Crystallography Crystal Structure studies for compounds 1 and 2. Crystals were

selected, sectioned as required, and mounted on plastic mesh with viscous oil and flash-

cooled to the data collection temperature. Diffraction data were collected on a Bruker-

Page 153: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

130

AXS APEX II Duo CCD diffractometer with graphite-monochromated Mo-Kα radiation

(λ=0.71073 Å). The data-sets were treated with SADABS absorption corrections based

on redundant multiscan data. The unit cell parameters and systematic absences in the

diffraction data were uniquely consistent for P21/c. The isomorphic structures were

solved using direct methods and refined with full-matrix, least-squares procedures on F2.

Unit cell parameters were determined by sampling three different sections of the Ewald

sphere. Nonhydrogen atoms were refined with anisotropic displacement parameters.

Hydrogen atoms were treated as idealized contributions. Structure factors and anomalous

dispersion coefficients are contained in the SHELXTL 6.12 program library.39

The

structures have been deposited at the Cambridge Crystallographic Data Centre under

CCDC 949353 & 949354

Chemical Vapor Deposition: All depositions were performed in a home built low

pressure hot-walled CVD apparatus.37

Si (1 0 0) wafers and SiO2 soda-lime glass

microscope slides were cleaned with piranha solution (H2SO4 and H2O2 in a 3:1 mixture)

for 20 minutes and air dried after rinsing with copious amounts of distilled water.

Substrates were allowed to equilibrate in a removable stainless steel boat at each furnace

temperature for 30 minutes under high vacuum. The external precursor container was

heated independently with resistive heating tape. Timing for each deposition experiment

began once the precursor container reached the setpoint temperature and finished when1

atm of N2 was admitted to the apparatus. The substrates were removed once cooled.

Film Characterization: Scanning electron microscopy (SEM, TESCAN) and

atomic force microscopy (AFM, Nanosurf) were used to study the surface morphology

and film thicknesses. The AFM software analysis package WSxM 5.0 was used for film

Page 154: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

131

thickness and roughness calculations.40

To determine film thickness the film was first

scratched with a knife and the step height was measured by AFM. A histogram (count of

feature heights) was extracted from the AFM data for a field of view that included

roughly equal areas of film and substrate along the scratch. The difference between the

two histogram maxima was then taken as the thickness of the film. Film thickness values

corroborated with values determined from SEM interrogation of cross-sections. Sheet

resistance was measured with a four-point probe. The elemental composition was

determined by XPS using a custom-built, ultra-high vacuum SPECS (GmbH) XPS

system (see Supporting Information). XPS spectra were collected after cycles of 2 min of

sputtering with Ar at 0.7 keV until a constant composition was obtained. Spectral fitting

and processing was performed using the CasaXPS Software Package. All high-resolution

scans and survey scans were fitted to a Shirley background and all component peaks

during the fitting process were generated by mixed Gaussian-Lorentz (GL) functions and

fit according to the Scofield-based relative sensitivity factors (RSFs) built into CasaXPS.

Thermal Decomposition Solution Studies: Solutions of 1 and 2 were prepared by

adding a known mass of compound to a known mass of C6D6. A drop of TMS was added

as an internal standard. The concentrations for 1 and 2 were 7.8 mM and 1.8 mM,

respectively. The solutions were frozen in heavy walled NMR tubes in liquid N2 and

flamed sealed under 100 mtorr dynamic vacuum. The isothermal oven was illuminated

with a 60 W incandescent light bulb and NMR tubes were wrapped with aluminum foil to

exclude light. 1H NMR spectra were measured on a 300 MHz Avance 3 every 24 h after

the tubes cooled to room temperature for 20 mins. The 2.5 ppm methylene peak in the 1H

NMR spectra was measured daily to track decomposition rates and products.

Page 155: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

132

Supplemental Information 5.6

Estimation of Vapour Pressure The procedure was followed as described in Ref.

34 with the modification that evaporation rates were measured from stepped isothermal

experiments. The Langmuir equation was used to relate experimentally determined

isothermal evaporation rates to vapour pressure:

𝑃 = 𝑑𝑚

𝑑𝑡√

𝑇

𝑀

√2𝜋𝑅

𝛼1 (1)

where; P = vapour pressure

T = isothermal temperature

dm/dt = evaporation rate determined from isothermal TGA

M = molecular mass

R = gas constant

α1 = vaporization coefficient

The vaporization coefficient, α1, accounts for the flowing gas environment of the

TG instrument. When considered along with √2𝜋𝑅, the parameter k = √2𝜋𝑅

𝛼1 is defined as

the material-independent part of Equation (1). The value for k for the TGA instrument

was determined from isothermal evaporation rates of benzoic acid and vapour pressure

values determined from Antoine constants (A = 7.454, B = 1820, C = 147.96). The value

for k was determined from the average of two stepped isothermal runs to be 65830 kg1/2

m s-1

K-1/2

. The stepped isothermal experiments were conducted between 60 - 120 °C

with 10 °C increments and a ramp rate of 40 °C/min was used between isothermal

temperatures.

To validate this method, we compared our estimated vapor pressure data of

Cu(tmhd)2 to known vapour pressure data (Colominas et al. J. Chem. Eng. Data 2001, 46,

446-450). Good agreement was obtained between these two sets of data. The temperature

Page 156: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

133

of 1 torr of vapour pressure was calculated to be 167 °C and Colominas et al. measured 1

torr of vapor pressure at 152 °C.

The stepped isothermal experiments for 1 and 2 were conducted between 130-190

°C with 10 °C increments and a ramp rate of 40 °C/min was used between isothermal

temperatures. A 1 cm Pt pan with a surface area of 0.785 cm2 was used for all

experiments. The calibration constant, k, and Equation (1) were used to convert the

isothermal evaporation rates to values for vapour pressure for 1 and 2 from which a 1 torr

temperature could be obtained by extrapolation.

XPS and Ar+-sputtering: Chemical composition analysis of the Au and Ag films

was carried out in a custom-built, ultra-high vacuum SPECS (GmbH) XPS system.

Samples were mounted to an iron sample holder and held in place using molybdenum

clips. For this study we used an Al Kα X-ray source operated at ~14 keV (26 mA) under

a base pressure of 1 x 10-10

Torr. Survey spectra (0-1000 eV) and high-resolution scans of

Au, Ag, C, N, and O regions were collected in SpecsLab2 (v. 2.7) software. Spectra were

collected at a fixed sample holder angle of 0o with the x-ray probe-to-sample distance of

~12 mm. Optical parameters of the PHOIBOS hemispherical analyzer 3500 (HSA3500)

and scanning parameters used in SpecsLab2 are found in the following table:

HSA3500 parameters scan mode (SpecsLab2)

entrance slit 7 mm x 20 mm scan parameter survey component

aperture medium energy step (eV) 0.2-0.4 0.05-0.1

exit slit open dwell time (s) 0.3 0.1-0.3

iris aperture 32 mm number of scans 1 2-5

lens mode medium pass energy (eV) 10 30

analysis mode fixed analyzer

transmission

Page 157: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

134

The films were subjected to Ar+-sputtering cycles which last 2 min/cycle at a base

pressure of 1 x 10-5

Torr of Ar and 0.7 kV filament potential. The sputtering depth of the

Ar+ is typically 10-20 Å and was used to remove impurities such as C, O, and N that may

have been initially present on the surface of the films. This would also yield the accurate

bulk composition of the pristine Au and Ag films. Spectral fitting and processing was

performed using the CasaXPS Software Package. All high-resolution scans and survey

scans were fitted to a Shirley background and all component peaks during the fitting

process were generated by mixed Gaussian-Lorentz (GL) functions and fit according to

the Scofield-based relative sensitivity factors (RSFs) built into CasaXPS.

Figure 5.12 XPS survey spectrum of Ag on Si(1 0 0) substrate as-deposited (blue), after

1 sputtering cycle (green), after 2 sputtering cycles (red), and after 3 sputtering cycles

(black). Ar+ sputtering cycles lasted 2 min and were done under base Ar pressures of 1 x

10-5

Torr.

Page 158: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

135

Figure 5.13 XPS survey spectrum of Au on Si (1 0 0) substrate as deposited (black), after

1 sputtering cycle (red), after 2 sputtering cycles (green), after 3 sputtering cycles (blue),

and after 4 sputtering cycles (cyan). Ar+ sputtering cycles lasted 2 min and were done

under Ar pressures of 1 x 10-5

Torr.

References 5.7

1 Weber, W. H.; McCarthy, S. L. Phys. Rev. B. 1975, 12, 5643.

2 Ozbay, E. Science 2006, 311, 189.

3 Doppelt, P. Coord. Chem. Rev. 1998, 178-80, 1785.

4 George, S. M. Chem. Rev. 2010, 110, 111.

5 Miikkulainen, V.; Leskelä, M.; Ritala, M.; Puurunen, R. L. J. Appl. Phys. 2013,

113, 021301.

6 (a) Zaera, F. Coor. Chem. Rev. 2013 doi: 10.1016/j.ccr2013.04.006, (b) Lei, Y.; Lu,

J.; Zhao, H.; Liu, B.; Low, K. –B.; Wu, T.; Libera, J. A.; Greely, J. P.; Chupas, P.

J.; Miller, J. T.; Elam, J. W. J. Phys. Chem. C 2013, 117, 11141, (c) Geyer, S. M.;

Methaapanon, R.; Shong, B.; Pianetta, P. A.; Bent, S. F. J. Phys. Chem. Lett. 2013,

4, 176.

Page 159: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

136

7 (a) Wenzel, T. J.; Williams, E. J.; Haltiwanger, R. C.; Sievers, R. E. Polyhedron

1985, 4, 369, (b) Martensson, P.; Carlsson, J.-O. J. Electrochem. Soc. 1998, 145,

2926.

8 Park, K. H.; Marshall, W. J. J. Am. Chem. Soc. 2005, 127, 9330.

9 (a) Li, Z. W.; Rahtu, A.; Gordon, R. G. J. Electrochem. Soc. 2006, 153, C787,(b)

Li, Z. W.; Barry, S. T.; Gordon, R. G. Inorg. Chem. 2005, 44, 1728, (c) Lim, B. S.;

Rahtu, A.;Gordon, R. G. Nat. Mater. 2003, 2, 749,(d) Lim, B. S.; Rahtu, A.; Park,

J. S.; Gordon, R. G. Inorg. Chem. 2003, 42, 7951.

10 Coyle, J. P.; Monillas, W. H.; Yap, G. P. A.; Barry, S. T. Inorg. Chem. 2008, 47,

683.

11 Park, J. W.; Jang, H. S.; Kim, M.; Sung, K.; Lee, S. S.; Chung, T.; Koo, S.; Kim, C.

G.; Kim, Y. Inorg. Chem. Commun. 2004, 7, 463.

12 Grushin, V. V.; Marshall, W. J. Adv. Synth. Catal. 2004, 346, 1457.

13 (a) Yuan, Z.; Dryden, N. H.; Vittal, J. J.; Puddephatt, R. J. Chem. Mater. 1995, 7,

1696, (b) Chiong, H. A.; Daugulis, O. Organometallics 2006, 25, 4054.

14 International Technology Road for Semiconductors; 2011; http://www.itrs.net/.

15 Kariniemi, M.; Niinistö, J.; Hatanpää, T.; Kemell, M.; Sajavaara, T.; Ritala, M.;

Leskelä, M. Chem. Mater. 2011, 23, 2901.

16 (a) Caldwell, J. D.; Glembocki, O. J.; Francisco, J. B.; Kariniemi, M. I.; Niinistö, J.

T.; Hatanpaa, T. T.; Rendell, R. W.; Ukaegbu, M.; Ritala, M. K.; Prokes, A. M.;

Hosten, C. M.; Leskelä, M. A.; Kasica, R. Opt. Express 2011, 19, 26056. (b)

Prokes, S. M.; Glembocki, O. J.; Cleveland, E.; Caldwell, J. D.; Foos, E.; Niinistö,

J.; Ritala, M. Appl. Phys. Lett. 2012, 100, 053106, (c) Cleveland, E. R.; Glembocki,

O.; Prokes, S. M. Proceedings of the SPIE – Nanoepitaxy: Materials and Devices

2012, 8467, 84670H/1, (d) Prokes, S. M.; Glembocki, O. J.; Cleveland, E.

Proceedings of the SPIE – Nanoepitaxy: Materials and Devices 2012, 8467,

84670F/1

17 Whitehorne, T. J. J.; Coyle, J. P.; Mahmood, A.; Monillas, W. H.; Yap, G. P. A.;

Barry, S. T. Eur. J. Inorg. Chem. 2011, 3240

18 (a) Shao, L. –Y.; Coyle, J. P.; Barry, S. T.; Albert, J. Opt. Mater. Express 2011, 1,

128, (b) Zhou, W.; Mandia, D. J.; Griffiths, M. B. E.; Bialiayeu, A.; Zhang, Y.;

Gordon, P. G.; Barry, S. T.; Albert, J. Opt. Express 2013, 21, 245

Page 160: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

137

19 (a) James, A. M.; Laxman, R. K.; Fronczek, F. R.; Maverick, A. W. Inorg. Chem.

1998, 37, 3785, b)Hitchcock, P. B.; Lappert, M. F.; Pierssens, L. J. -M. Chem.

Commun. 1996, 1189, (c) Bunge, S. D.; Just, O.; Rees, W. S. Jr. Angew. Chem. Int.

Ed. 2000, 39, 3082.

20 Grodzicki, A.; Łakomska, I.; Piszczek, P.; Szymańska, I.; Szłyk, E. Coord. Chem.

Rev. 2005, 249, 2232.

21 Bollmann, D.; Merkel, R.; Klumpp, A. Microelectron. Eng. 1997, 37-8, 105

22 Norman, J. A.T.; Perez, M.; Schulz, S. E.; Waechtler, T. Microelectron. Eng. 2008,

85, 2159

23 Gao, L.; Härter, P.; Linsmeier, Ch.; Wiltner, A.; Emling, R.; Schmitt-Landsiedel,

D. Microelectron. Eng. 2005, 82, 296

24 Chi, K.-M.; Lu, Y.-H. Chem. Vap. Dep. 2001, 7, 117.

25 Yuan, Z.; Dryden, N. H.; Li, X.; Jagadese, J. V.; Puddephatt, R. J. J. Mater. Chem.

1995, 5, 303.

26 Szlyk, E.; Piszczek, P.; Lakomska, I.; Grodzicki, A.; Szatkowski, J.; Blaszczyk, T.

Chem. Vap. Dep. 2000, 6, 105.

27 (a) Banaszak Holl, M. M.; Seidler, P. F.; Kowalczyk, S. P.; McFeely, F. R. Inorg.

Chem. 1994, 33, 510, (b) Jansen, F.; Kruck, T. Adv. Mater. 1995, 7, 298, (c) Au, R.

H. W.; Puddephatt, R. J. Chem. Vap. Dep. 2007, 13, 20.

28 (a) Larson, C. E.; Baum, T. H.; Jackson, R. L. J. Electrochem. Soc. 1987, 134, 266,

(b) Bessonov, A. A.; Morozova, N. B.; Gelfond, N. V.; Semyannikov, P. P.;

Trubin, S. V.; Shevtsov, Yu. V.; Shubin, Yu. V.; Igumenov, I. K. Surf. Coat.

Technol. 2007, 210, 9099, (c) Bessonov, A. A.; Morozova, N. B.; Gelfond, N. V.;

Semyannikov, P. P.; Baidina, I. A.; Trubin, S. V.; Shevtsov, Yu. V.; Igumenov, I.

K. J. Organomet. Chem. 2008, 693, 2572, (d) Parkhomenko, R. G.; Morozova, N.

B.; Zharkova, G. I.; Shubin, Y. V.; Trubin, S. V.; Kriventsov, V. V.; Kuchumov, B.

M.; Koretskaya, T. P.; Igumenov, I. K. Chem. Vap. Dep. 2012, 18, 336, (e)

Parkhomenko, R. G.; Turgambaeva, A. E.; Morozova, N. B.; Trubin, S. V.;

Krisyuk, V. V.; Igumenov, I. K. Chem. Vap. Dep. 2013, 19, 38.

29 Coyle, J. P.; Johnson, P.; DiLabio, G.; Müller, J.; Barry, S. T. Proceedings of the

AVS Atomic Layer Deposition Conference 2009.

Page 161: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

138

30 Coyle, J. P.; Johnson, P.A.; DiLabio, G. A.; Barry, S. T.; Müller, J. Inorg. Chem.

2010, 49, 2844.

31 Coyle, J. P.; Kurek, A.; Pallister, P. J.; Sirianni, E. R.; Yap, G. P. A.; Barry, S. T.

Chem. Commun. 2012, 48, 10440.

32 Ziffle, L. C.; Kenney, A. P.; Barry, S. T.; Müller, J. Polyhedron 2008, 27, 1832.

33 JCPDS Card File No. 00-004-0784 (Au) and 01-089-3722 (Ag).

34 Coyle, J. P.; Pallister, P. J.; Kurek, A.; Sirianni, E. R.; Yap, G. P. A.; Barry, S. T.

Inorg. Chem. 2013, 52, 910.

35 Kunte, G. V.; Shivashankar, S. A.; Umarji, A. M. Meas. Sci. Technol. 2008, 19,

025704.

36 (a) Ma, Q.; Guo, H.; Gordon, R. G.; Zaera, F. Chem. Maters. 2011, 23, 3325, (b)

Kim, T.; Yao, Y.; Coyle, J. P.; Barry, S. T.; Zaera, F. Chem. Maters. 2013, 25,

3630.

37 Gordon, P. G.; Ward, M. J.; Heikkila, M. J.; Monillas, W. H.; Yap, G. P. A.; Ritala,

M.; Leskelä, M.; Barry, S. T. Dalton Trans. 2011, 40, 9425.

38 Usón, R.; Laguna, A.; Laguna, A. M.; Briggs, D. A.; Murray, H. H.; Fackler, J. P.

Inorg. Synth. 1989, 26, 85.

39 Sheldrick, G.M. Acta Cryst. 2008, A64, 112-122.

40 Horcas, I.; Fernandez, R.; Gomez-Rodriguez, J. M.; Colchero, J.; Gomez-Herrero,

J.; Baro, A. M. Rev. Sci. Instrum. 2007, 78, 013705.

Page 162: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

139

Deposition of Copper by Plasma-Enhanced Atomic Layer 6 Chapter:

Deposition Using a Novel N-Heterocyclic Carbene Precursor

Modified from original manuscript published as:

Jason P. Coyle1, Gangotri Dey2, Eric R. Sirianni3, Marianna L. Kemell4, Glenn P. A. Yap3, Mikko

Ritala4, Markku Leskelä4, Simon D. Elliott2, Sean T. Barry1 “Deposition of Copper by Plasma-

Enhanced Atomic Layer Deposition Using a Novel N-Heterocyclic Carbene Precursor” Chem.

Mater. 2013 25, 1132-1138

1 Department of Chemistry, Carleton University, 1125 Colonel By Drive, Ottawa, K1S 5B6,

Canada.

2 Tyndall National Institute, University College Cork, Dyke Parade, Cork, Ireland

3 Department of Chemistry & Biochemistry, University of Delaware, Newark, DE 19716, United

States

4 Laboratory of Inorganic Chemistry, Department of Chemistry, University of Helsinki P.O. Box

55, FI-00014 Helsinki, Finland

Abstract 6.1

Two novel N-heterocyclic carbene (NHC)-containing copper(I) amides are

reported as atomic layer deposition (ALD) precursors. 1,3-diisopropyl-imidazolin-2-

ylidene copper hexamethyldisilazide (1) and 4,5-dimethyl-1,3-diisopropyl-imidazol-2-

ylidene copper hexamethyldisilazide (2) were synthesized and structurally characterized.

The thermal behaviour of both compounds was studied by thermogravimetric analysis

(TGA), and they were both found to be reasonably volatile compounds. Compound 1 had

no residual mass in the TGA and showed long-term stability at temperatures as high as

130 °C, while 2 had a residual mass of 7.4 %. Copper metal with good resistivity was

deposited using 1 by plasma-enhanced atomic layer deposition. The precursor

demonstrated self-limiting behaviour indicative of ALD, and gave a growth rate of 0.2

Å/cycle. Compound 2 was unsuccessful as an ALD precursor under similar conditions.

Density functional theory calculations showed that both compounds adsorb dissociatively

Page 163: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

140

onto a growing copper film as long as there is some atomic roughness, via cleavage of the

Cu-carbene bond.

Introduction 6.2

Copper metal remains an interesting topic for chemical vapour deposition (CVD)

and atomic layer deposition (ALD) due to its use in microelectronics, primarily as an

interconnect.1 Several potential copper(I) and copper(II) precursors have been reported

for chemical vapor deposition (CVD) and atomic layer deposition (ALD), including β-

diketonates,2 β-diketiminates,

3 amidinates,

4 guanidinates,

5 aminoalkoxides,

6 and

pyrrolylaldiminates.7 Of these precursors, the exclusively N-bonded ligands are

interesting due to their lack of Cu-O bonds, making them less susceptible to oxygen

inclusion in the deposited copper film as well as in the barrier and adhesion layers.

ALD has been proposed as an alternative method to CVD for depositing

conformal, ultra-thin films at comparatively lower temperatures. ALD is similar to CVD

except that the substrate is sequentially exposed to one reactant at a time, or one dose of a

reactant at a time. Conceptually, it is a simple process: a first reactant is introduced to a

heated substrate whereby it forms a monolayer on the surface of the substrate. Excess

reactant is pumped out (e.g., evacuated). Next a second reactant is introduced and reacts

with the existing monolayer to form a sub-monolayer of a desired reaction product

through a self-limiting surface reaction. The process is self-limiting since the deposition

reaction halts once the initially adsorbed (physisorbed or chemisorbed) monolayer of the

first reactant has fully reacted with the second reactant. Finally, the excess second

reactant is evacuated. This sequence constitutes one deposition cycle. The desired film

thickness is obtained by repeating deposition cycles as necessary. As is apparent, the

Page 164: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

141

sequential layer-by-layer nature of ALD has the disadvantage of being slower than some

other deposition techniques. However it is this cycle of building up highly uniform

layers one at a time that allows ALD to produce films of a surface uniformity,

smoothness and thinness that is impossible to achieve with other techniques. This makes

ALD uniquely valuable in demanding coating applications. In the specific application of

ALD used for this study, the “second reactant” in this case is a hydrogen plasma,

generated remotely from the growing surface from dihydrogen carried by argon. This

plasma is screened by a grounded grid, filtering out ions from the plasma, and permitting

only the radicals (and light) produced in the plasma to impinge on the surface. The role

of the the hydrogen plasma is to scour off the ligand system, as well as reducing the

copper surface species to metal. Given the complex nature of the plasma, the mechanistic

reaction at the surface is likely complex. An excellent review of plasma ALD processes

can be found here.8

It is interesting that copper amides have not been prevalent precursors for ALD.

It is known that copper(I) amides typically produce a tetrameric structure,9 and copper(I)

amides are more thermally stabile than alkyl or alkoxo species.10

Thus, it has been

difficult to isolate a thermally stable copper amide precursor that exhibits sufficient

volatility to be considered for CVD or ALD. However, monomeric copper(I) species are

well-studied in catalysis. Specifically, copper(I) NHCs are well-known to exhibit good

thermal stability during C-H bond activation11

and can drastically increase the thermal

stability in sensitive Cu(I) species.12,13

Thus, the synthesis and thermal characterization

of copper(I) amides stabilized by NHCs was undertaken to examine their suitability as

Page 165: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

142

ALD precursors. This design strategy is common for group 11 precursors, and recent

success has been shown for the plasma enhanced ALD of Ag films.14

Figure 6.1 The structures of 1,3-diisopropyl-imidazolin-2-ylidene copper

hexamethyldisilazide (1) and 4,5-dimethyl-1,3-diisopropyl-imidazol-2-ylidene copper

hexamethyldisilazide (2).

Herein is reported novel copper(I) NHCs: 1,3-diisopropyl-imidazolin-2-ylidene

copper hexamethyldisilazide (1) and 4,5-dimethyl-1,3-diisopropyl-imidazol-2-ylidene

copper hexamethyldisilazide (2) (Figure 6.1). The choice of ligands was paramount for

the design of this new copper precursor. Preliminary screening showed that

hexamethyldisilazide (-N(SiMe3)2) provided excellent thermal stability to Cu(I), where

alkyl amides are known to allow plating of copper metal.10

It was less clear from the

outset whether an unsaturated NHC (imidazol-2-ylidene) or saturated NHC (imidazolin-

2-ylidene) would allow for better precursor properties and for better metal deposition.

Preliminary screening of unsaturated NHCs showed that an imidazol-2-ylidene with a

methyl-substituted backbone provided a more thermally stable copper compound than an

unsubstituted imidazol-2-ylidene. Preliminary screening showed backbone substitution

of imidazolin-2-ylidenes proved to be unnecessary as such NHCs afforded copper

compounds with sufficient thermal stability. Interestingly, our preliminary screening led

Page 166: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

143

us to choose NHCs with different stabilities towards dimerization; the dimer from the

carbene in 2 is unknown, whereas the dimer from the carbene in 1 is a volatile olefin.15

Some Cu(I) precursors are well known to undergo disproportionation reactions to

Cu(0) and Cu(II), which has been exploited in the CVD of copper metal films.16

This

process relies on the clean purging from the deposition zone of the Cu(II) product along

with any stabilizing Lewis base employed in the Cu(I) precursor. Cu(II)

hexamethyldisilazide compounds are unknown and Cu(II) amide compounds are

exceptionally rare.17

The attempted synthesis of Cu[N(SiMe3)2]2 results in the isolation of

[CuN(SiMe3)2]4.18

CVD of copper metal films from [CuN(SiMe3)2]4 have been reported

at 200°C under a flow of H2 without any indication of a disproportionation component to

film growth.18

Both of the NHCs used in 1 and 2 are volatile at room temperature when

not coordinated; however their affinities for a copper surface are investigated herein.

Additionally, explicit atomic-scale insight into ALD chemistry has been obtained

through simulations using Density Functional Theory (DFT).19

Most DFT studies have

been related to the ALD of binary compounds such as HfO220

and Al2O3,21

but there are

relatively few simulations on the ALD of pure metals (e.g. Ni22

and Co23

). Possible Cu

ALD reactions have been computed by Mårtensson et al. for CuCl as the precursor and

H224

as the reducing agent. The formation of Cu from amidinate25

and β-diketonate26,27

based precursors has also been simulated. Recently, Dey et al. have computed a detailed

mechanism for Cu ALD using ZnEt2 as the reducing agent,28

following experiments by

Lee et al.29

Here we use DFT to compare the probable adsorption mechanism of the

carbene-based Cu precursors 1 and 2.

Page 167: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

144

Results and Discussion 6.3

Both compounds can be made by simple salt metathesis from the NHC copper

chloride and Et2O·LiN(SiMe3)2 . The resulting 1H spectra were simple and reflected the

expected formulations in both cases. Compound 1 easily underwent sublimation under

reduced atmosphere at 90 °C, and was sublimed quantitatively. It melted at 51 °C, which

is beneficial for a vapour phase precursor: having the precursor as a liquid during the

deposition process ensures a uniform production of vapour pressure. Thermogravimetric

analysis (TGA) showed the onset of volatility at 91 °C and a residual mass of 0 % (Figure

6.2, black trace). Compound 2 could also be quantitatively sublimed at 95 °C and had a

melting point of 119 °C. TGA showed an onset of volatility at 87 °C, but with a residual

mass of 7.4 %. Since the mass of copper in 2 comprises 15.72 % of the total molecular

mass, this compound was possibly undergoing volatilization and decomposition over the

thermal range of the TGA.

Figure 6.2 Thermogravimetric analyses and evaporation rates of 1 (black) and 2 (grey)

run at 10 °C/min ramp rate, with 10 °C increments for the stepped isotherm used to

determine evaporation rate.

Page 168: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

145

It was possible to isolate crystals of both 1 and 2 that were sufficient for structural

analysis (Figure 6.3, Table 6.1). In both cases, the copper is in a linear geometry with the

ligands staggered and roughly orthogonal. The Cu-N bonds (1.84 Å for 1 and 1.87 Å for

2) are shorter than reported for the copper(I) hexamethyldisilazide tetramer (1.92 – 1.93

Å),18

but similar to copper alkyl amide compounds.9 The longer amide contact in 2 might

be due to the steric bulk of the backbone methyl groups forcing the carbene's isopropyl

groups to orient toward the amide moiety, in turn forcing back the amide group. The

copper-carbon bonds fall in the range of other monomeric, linear N-bonded Cu-NHC

complexes,30,12

suggesting that the shortened Cu-N bond might be due to enhanced π-

donation to the copper. This also suggests that the copper amide bond might be stabilized

to cleavage upon adsorption of the compound at a growing copper surface, suggesting

that the carbene will be lost upon chemisorption.

Figure 6.3 The X-ray structure of 1 (left) and 2, (right), with H-atoms and minor

disordered contributions omitted for clarity and at 30 % probability ellipsoids.

Page 169: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

146

Table 6.1 Selected bond lengths and bond angles for the structures of 1 and 2.

Compound 1 Compound 2

experimental computational experimental computational

selected bond lengths (Å)

Cu–N3 1.836(4) 1.869 Cu–N3 1.870(2) 1.869

Cu–C1 1.870(5) 1.897 Cu–C1 1.881(2) 1.897

N1–C1 1.330(7) 1.356 N1–C1 1.360(3) 1.367

N1–C2 1.472(7) 1.470 N1–C5 1.404(3) 1.397

N2–C1 1.336(6) 1.356 N2–C1 1.365(3) 1.372

N2–C3 1.444(9) 1.471 N2–C7 1.394(3) 1.399

Si1–N3 1.680(6) 1.742 N3–Si2 1.692(2) 1.742

Si2–N3 1.701(5) 1.742 N3–Si1 1.697(2) 1.741

C2–C3 1.531(12) 1.538 C5–C7 1.338(4) 1.384

selected bond angles (deg)

N3–Cu–C1 179.2(2) 178.3 N3–Cu–C1 178.60(9) 175.5

C1–N1–C2 114.2(5) 112.1 C1–N1–C5 111.0(2) 111.4

C1–N2–C3 114.7(6) 112.5 C1–N2–C7 111.6(2) 111.4

Si1–N3–Si2 128.2(3) 128.2 Si2–N3–Si1 131.26(13) 128.1

Si1–N3–Cu 116.5(3) 116.0 Si1–N3–Cu 113.19(11) 113.0

Si2–N3–Cu 115.3(3) 115.1 Si2–N3–Cu 111.21(11) 113.0

N1–C1–N2 106.6(5) 107.9 N1–C1–N2 103.9(2) 104.5

N1–C1–Cu 127.0(4) 128.0 N1–C1–Cu 127.26(19) 130.6

N2–C1–Cu 126.3(5) 128.0 N2–C1–Cu 128.88(19) 130.6

A “stepped isotherm” TGA was employed to establish the evaporation rate and

vapour pressures of these compounds. A stepped isotherm is a thermogravimetric

experiment where the temperature is ramped by 10 °C and held for 10 minutes while the

compound volatilizes; the number of steps gives the number of data points from which a

Clausius-Clapeyron curve can be constructed. This experiment can be used to relate the

mass lost as vapour to the Langmuir equation, to establish vapour pressure as a function

Page 170: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

147

of temperature.31

Compound 1 was shown to be more volatile at lower temperatures, and

to have 1 Torr of vapour pressure at 149 °C (using benzoic acid as a standard). 32

Compound 2 had a slightly lower volatility, and gave 1 Torr of vapour pressure at 158

°C. However, both of these compounds can be expected to give reasonably high vapour

pressures at normal bubbler temperatures, and the similarity of the slopes of their

evaporation curves suggests that they experience similar intermolecular attraction during

evaporation.

Since the TGA of 1 showed no thermal decomposition, a thermal “delivery

stability” test was performed to determine the long-term stability of this compound at

reasonable bubbler temperatures. It is desirable for ALD precursors to demonstrate

stability under bubbler conditions to ensure predictable and consistent vapour pressures

delivered with each pulse. The thermal stress test used a stainless steel vessel which was

heated in an isothermal oven. Samples were taken using a glovebox every 48 h for 2

weeks, and the samples were analysed by TGA and 1H NMR. A 90 °C oven temperature

was chosen as this was the delivery temperature in plasma-enhanced (PE) ALD

experiments described below. The TGA showed an increasing trend in residual mass

from 2 % to 3 % over two weeks, which is an excellent thermal stability at delivery

temperatures. The 1H NMR spectra measured on day 1 and day 14 both showed only

peaks for 1. This delivery stability test was repeated using an oven temperature of 130

°C. Sampling over two weeks showed the residual mass increasing from 1 % to 3 %.

Again, 1H NMR spectra corroborated the excellent thermal stability displayed at 130 °C.

A delivery stability test was not performed for 2, as decomposition was evident from

preliminary TGA.

Page 171: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

148

Compound 1 was successful at depositing copper metal using PE-ALD. A typical

experiment saw 0.3 - 0.5 g of 1 loaded into a Beneq TFS 200 reactor equipped with a

capacitively coupled plasma source. The substrate was heated to 225 °C and the

precursor was heated to 90 °C to ensure sufficient vapour of 1 reaching the deposition

chamber. A pulse of 1 was followed by a 3 s purge with nitrogen gas, alternating with a

6 s pulse of hydrogen plasma and a second purge. Varying the pulse length of 1 allowed

a saturation curve to be collected (Figure 6.4). The growth rate plateaued at 0.2 Å/cycle

after

Figure 6.4 ALD saturation curve for 1 as the pulse length of 1 was varied.

4 seconds, corresponding to about 10 % of a monolayer of Cu. ALD-grown copper has

been reported with growth rates of 0.12 Å/cycle (on Ru),33

0.18Å/cycle ,34

and 0.90

Å/cycle35

, showing this growth rate to be within this range. Energy dispersive X-ray

spectroscopy (EDS) showed the resulting material to be copper metal, with some minor

carbon impurities (<5%). Since the thicknesses were measured using the k-ratios from

EDS, the growth from 1 s and 2 s pulse lengths gave no thickness. However, scanning

electron microscopy showed nucleation of copper nanoparticles (Figure 6.5). It was

Page 172: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

149

obvious that the deposited copper was crystalline over all deposition ranges, and X-ray

diffraction showed typical copper signals, and demonstrated the absence of copper oxide

crystalline phases. Many of the deposited films were too thin and non-continuous for

resistivity measurements, but the film deposited with a 5 s pulse had a thickness of 35 nm

and gave a resistivity of 11.23 μΩ·cm. This is not unusual for the deposition of copper

metal on silicon: the high mobility of copper atoms on the growing surface result in an

island growth mechanism that causes non-uniformity.

Figure 6.5 Scanning electron micrographs of deposited copper films. (a) Plan view of

copper nanoparticles deposited using a 1 s pulse length. (b) Plan view of crystalline

copper deposited using a 4 s pulse length. (c) Plan view of crystalline copper deposited

using a 6 s pulse length. (d) A profile of crystalline copper deposited using a 6 s pulse

length.

Page 173: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

150

Compound 2 could not be used under any tested conditions as a copper metal

precursor. The resulting depositions were not metallic, but showed an interference colour

pattern similar to non-uniform deposition of a transparent material. A typical “blank”

experiment was performed where by the hydrogen pulse was not activated to plasma. No

film growth was observed during this experiment for either 1 or 2. The difference in the

deposition results between 1 and 2 was attributed to the NHC, since the rest of the

molecule is unchanged.

DFT calculations were carried out on these precursors in the gas phase and

adsorbed to model copper surfaces. The computed structures were in good agreement

with the X-ray structural analysis, with all bond lengths agreeing within 5 pm (Table 6.1).

The dissociation energy of each ligand from the copper centre was calculated to

determine which bond was likely to break upon chemisorption at a copper surface. The

chemical equations considered were heterolysis of the amide bond (1), homolysis of the

amide bond (2), and loss of the NHC (3):

NHC-Cu(I)-N(SiMe3)2 → [NHC-Cu(I)]+ + [N(SiMe3)2]

- (1)

NHC-Cu(I)-N(SiMe3)2 → [NHC-Cu(0)] + [N(SiMe3)2]• (2)

NHC-Cu(I)-N(SiMe3)2 → NHC + Cu(I)-N(SiMe3)2 (3)

In compounds 1 and 2, it was found that the copper-nitrogen bond (Eqs. 1 and 2)

was much stronger than the copper-C bond to NHC (Eq. 3), (646 and 428 kJ/mol vs. 293

kJ/mol for 1; 636 and 427 kJ/mol vs. 298 kJ/mol for 2). Thus, the amide will remain

bound to the Cu atom during adsorption, which likely forms new Cu-Cu bonds with the

Page 174: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

151

surface, while the carbene may dissociate from the adsorbing molecule and bond

separately to the surface or evaporate.

Figure 6.6 Optimized geometries of (a) 2 molecularly physisorbed on a smooth Cu (111)

surface; (b) CuN(SiMe3)2 chemisorbed on the smooth surface; (c) NHC from 2

chemisorbed onto a rough surface; (d) NHC from 2 physisorbed on the smooth surface.

The precursors were brought to a model copper surface and relaxed with DFT in

order to determine their adsorption energy (∆Ead). In both cases, the Cu atom of the

precursor optimized to a distance of 5.4 Å from the nearest surface Cu atom (Figure 6.6).

The precursor contacted the surface via the alkyl substituent of the -N(SiMe3)2, with a

shortest Cu-H distance of 2.4 Å to the nearest surface Cu atom. These are non-bonded

distances, indicative of molecular physisorption. We can see from the DFT energetics

(Table 6.2) that the precursors have weak molecular adsorption to the surface for both 1

and 2, although there is some uncertainty in this value because of the poor description of

physisorption by DFT. Explicit inclusion of van der Waals interactions in the DFT

functional may give a more accurate value36,37,

but the use of such functionals for

organometallic reagents adsorbed onto metal surfaces is not yet well established and

hence is beyond the scope of our study.38

Page 175: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

152

It appears that steric hindrance in the -N(SiMe3)2 moiety prevents the

coordinatively unsaturated Cu, C and N atoms of the precursor from coming close to the

surface (Figure 6.6). The only pathway to chemisorption is therefore through dissociation

of the precursor at the Cu-NHC bond. The adsorption energies show that the carbene of 1

and 2 can adsorb to the smooth surface with comparable energies (Table 6.2).

Table 6.2 Computed Adsorption Energy ΔEad (kJ/mol) of the Precursors and Their

Probable by-Products on Two Surface Models - Cu55 with a Smooth (111) Surface and

Cu56 with One Extra Atom Making the Surface Rough.a

adsorbate surface model structure compound 1 compound 2

Cu(NHC)[N(SiMe3)2] smooth Cu55 Fig 6.6a (-174) (-174)

NHC smooth Cu55 Fig 6.6d (-61) (-83)

NHC rough Cu56 Fig 6.6c -255 -256

NHC (dimer)

smooth Cu55 (-113) (-101)

Cu(I)(NHC)+ smooth Cu55 Fig 6.6c -364 -353

[N(SiMe3)2]- smooth Cu55 -378

[N(SiMe3)2]- rough Cu56 Fig 6.6b -385

Cu(I)[N(SiMe3)2] smooth Cu55 Fig 6.6b -308

aValues for physisorption are in brackets because of the limited accuracy of the PBE

functional in describing van der Waals interactions.

For a smooth copper surface, the adsorption energies are low and - consistent with this -

the computed distances indicate that no chemical bonds are formed to the Cu surface.

However, when a rough surface (modeled by an additional copper(I) adatom) is

considered, the NHC ligands bind to this surface site with adsorption energies that are

comparable to those of the Cu-N(SiMe3)2 moiety. The DFT data do not show any

significant difference between the saturated carbene (from 1) and unsaturated carbene

(from 2) in terms of energetics of dissociation or adsorption during the Cu pulse. This

Page 176: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

153

indicates that differences between the ALD chemistry of these two precursors arise after

the Cu pulse, probably during the plasma H2 pulse. Further studies are under way to

determine the differences in the surface chemistry of these two compounds.

Conclusion 6.4

Two novel NHC-containing compounds 1,3-diisopropyl-imidazolin-2-ylidene

copper hexamethyldisilazide (1) and 4,5-dimethyl-1,3-diisopropyl-imidazol-2-ylidene

copper hexamethyldisilazide (2) were synthesized and structurally characterized.

Compound 1 was found to have excellent volatility and thermal stability over an

extended period of time. It was successfully employed as an ALD precursor using

hydrogen plasma as a reducing agent. The deposited films had a growth rate of 0.2

Å/cycle and were crystalline. The films showed good resistivity.

Compound 2 showed excellent volatility but poorer thermal stability than 1.

Under similar conditions to the ALD of 1, it did not afford a copper metal film. DFT

studies of both precursors showed good dissociative chemisorption to a copper surface,

with cleavage of the precursor at the carbene-copper bond, indicating similar surface

chemistry during the Cu precursor pulse in ALD.

Experimental 6.5

General Considerations: All manipulations involving the synthesis and handling

of copper(I) compounds were performed in an MBraun Labmaster™ 130 Dry box

(mBraun, Stratham, NH, U.S.A.) under a nitrogen atmosphere. NMR spectra were

recorded on a 400 MHz Bruker AMX spectrometer. NMR spectra were measured in C6D6

and were referenced against residual protonated solvent. 1,3-diisopropyl-imidazolin-2-

Page 177: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

154

ylidene copper chloride was prepared from a literature method substituting imidazolinium

tetrafluoroborate for imidazolinium chloride.39

4,5-dimethyl-1,3-diisopropyl-imidazol-2-

ylidene copper chloride was prepared by following established literature methods for

NHC CuCl.40

4,5-dimethyl-1,3-diisopropyl-imidazol-2-ylidene41

and 1,3-diisopropyl-

imidazolinium chloride42

were prepared according to literature. The diethyl ether adduct

of lithium hexamethyldisilazide was prepared according to literature.43

All reagents were

purchased from Sigma Aldrich (Oakville, Ontario, Canada) and used as received. All

solvents were purchased as ACS grade and purified from an Mbraun Solvent Purifier

System.

1,3-diisopropyl-imidazolin-2-ylidene copper hexamethyldisilazide (1): 1,3-

diisopropyl-imidazolin-2-ylidene copper chloride (4.456 g, 17.52 mmol) was partially

dissolved in 130 mL of toluene and cooled in the glove box freezer to -35 ºC before use.

In a separate flask, Et2O·LiN(SiMe3)2 (4.248 g, 17.6 mmol) was dissolved in 70 mL of

toluene. The amide solution was added dropwise over the course of a hour and the

cloudy solution was stirred for 24 h, after which the solution was filtered and the

insoluble material was washed with 3 × 10 mL of toluene. The washings were combined

with the filtrate and volatiles were stripped off under reduced pressure. The crude product

was purified by sublimation (Tsub = 90 °C, 35 mTorr) using a dry ice/acetone cold finger

and collected as a colourless solid (6.322 g, 95 %); m.p. 49-51 °C. 1H NMR (400 MHz,

C6D6): δ 4.46 [sept, 2H, NCH(CH3)2], δ 2.50 [s, 4H, N(CH2)2N], δ 0.81 [d, 12H,

NCH(CH3)2], δ 0.54 [s, 18H, N(Si(CH3)3)2]. 13

C NMR (100 MHz, C6D6): δ 200.39

[NCN], δ 51.16 [NCH(CH3)2], δ 41.91 [N(CH2)2N], δ 20.68 [NCH(CH3)2], δ 7.20

[N(Si(CH3)3)2]. HRMS (EI) m/z calcd for C15H36N3Si2Cu M+ 377.1744, found 377.1763.

Page 178: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

155

4,5-dimethyl-1,3-diisopropyl-imidazol-2-ylidene copper hexamethyldisilazide (2):

Compound 2 was prepared in an analogous manner as compound 1 substituting: 4,5-

dimethyl-1,3-diisopropyl-imidazol-2-ylidene copper chloride (0.518 g, 1.85 mmol)

partially dissolved in 15 mL of toluene, Et2O·LiN(SiMe3)2 (0.449 g, 1.86 mmol)

dissolved in 8 mL of toluene. Compound 2 was isolated by sublimation (Tsub = 95 ºC, 25

mTorr) as a white solid (0.630 g, 84.0%); m.p. 119 ºC. 1H NMR (400 MHz, C6D6): δ

4.08 [sept, 2H, NCH(CH3)2], δ 1.41 [s, 6H, N(CCH3)2N], δ 1.37 [d, 12H, NCH(CH3)2],

δ 0.59 [s, 18H, N(Si(CH3)3)2]. 13

C NMR (100 MHz, C6D6): δ 173.21 [NCN], δ 123.08

[N(CCH3)2N] , δ 50.67 [NCH(CH3)2], δ 24.02 [NCH(CH3)2], δ 8.80 [N(CCH3)2N], δ

7.12[N(Si(CH3)3)2]. HRMS (EI) m/z calcd for C17H38N3Si2Cu M+ 403.1900, found

403.1924.

Computational Study: The ground state electronic wave function of each

molecule was calculated self-consistently within Kohn-Sham DFT using the

TURBOMOLE suite of quantum chemical programs.44,45

The Perdew-Burke-Ernzerhof

functional46

with the resolution-of-the-identity approximation47,48

and an all-electron

valence double-zeta with polarization def-SV(P) basis set49

was considered the most

suitable level of calculation. No basis set superposition error correction was required for a

basis of this size. An even larger def-TZV(P)47

basis set gives reaction energies that

agree to less than 10%, but are an order of magnitude more costly in computational time.

Structures are relaxed using DFT with no constraints, except to stop adsorbates drifting

towards the edge of the cluster. All the neutral Cu(I) carbene precursor molecules are

closed shell compounds. A 55 copper atom cluster of C3v symmetry, which is in the shape

of a coin (Cu55), is used as a model of the (1 1 1) surface to see the effect of adsorption of

Page 179: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

156

various copper precursors. A rough surface has been generated by the addition of one Cu

atom (Cu56). The copper coin is an open shell system with the HOMO LUMO energy

difference of <2 kJ/mol. NPA50

has been carried out in order to obtain a qualitative

understanding of the charge distribution .

Crystallography: X-ray structural analysis: Crystals were selected and mounted

on plastic mesh using viscous oil flash-cooled to the data collection temperature. Data

were collected on a Brüker-AXS APEX CCD diffractometer with graphite-

monochromated Mo-Kα radiation (λ=0.71073 Å). Unit cell parameters were obtained

from 60 data frames, 0.3º ω, from three different sections of the Ewald sphere. The

systematic absences in the data and the unit cell parameters were uniquely consistent to

P21/n. The data-sets were treated with absorption corrections based on redundant

multiscan data. The structures were solved using direct methods and refined with full-

matrix, least-squares procedures on F2. In 1, one isopropyl and both trimethylsilyl

groups, and in 2, one trimethylsilyl group, were rotationally disordered with

1(isopropyl:trimethyl:tri-methyl):2(isopropyl)::88/12:63/37:60/40:51/49 refined site

occupancies. Chemically equivalent bond distances and angles in the disordered group

were constrained to average values and with equal atomic displacement atomic parameter

restraints on equivalent atoms. All atoms were treated in 1 were treated with rigid bond

restraints. All non-hydrogen atoms were refined with anisotropic displacement

parameters. All hydrogen atoms were treated as idealized contributions. Atomic

scattering factors are contained in the SHELXTL 6.12 program library.51

PE ALD: Copper thin films were deposited on silicon (100) substrates in a Beneq TFS-

200 ALD-reactor, capable of depositing on 200 mm wafers, with a remote plasma

Page 180: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

157

configuration.14b

Plasma was generated with capacitive coupling with a 13.56 MHz rf

power source. The plasma power was 170 W. The distance between the substrate and the

grid, which was the bottom electrode, was 4 cm. Plasma activated hydrogen was used as

the reducing agent. Hydrogen gas (99.999%, AGA) was mixed with argon (99.999%,

AGA) to ensure plasma ignition. In general, the hydrogen flow was 20 sccm and the

argon plasma gas flow 140 sccm. The hydrogen flow was not pulsed because no reaction

between the precursor and molecular hydrogen was noticed at the applied growth

temperatures. Argon carrier gas flow was typically 330 sccm. Gases were purified on-

site before mixing with Aeronex GateKeeper and Entergris GateKeeper purifiers.

References6.6

1 International Technology Roadmap for Semiconductors; 2011; http://www.itrs.net/.

2 (a) Chen, T. Y.; Omnes, L.; Vaisserman, J.; Doppelt, P. Inorg. Chim. Acta. 2004,

357, 1299, (b) Bollmann, D.; Merkel, R.; Klumpp, A. Microelectron. Eng. 1997, 37-

8, 105, (c) Lagalante, A. F.; Hansen, B. N.; Bruno, T. J.; Sievers, R. E. Inorg. Chem.

1995, 34, 5781 (d) Wenzel, T. J.; Williams, E. J.; Haltiwanger, R. C.; Sievers, R. E.

Polyhedron 1985, 4, 369.

3 Park, K. H.; Marshall, W. J. J. Am. Chem. Soc. 2005, 127, 9330.

4 (a)Li, Z. W.; Rahtu, A.; Gordon, R. G. J. Electrochem. Soc. 2006, 153, C787, (b) Li,

Z. W.; Barry, S. T.; Gordon, R. G. Inorg. Chem. 2005, 44, 1728, (c) Lim, B. S.;

Page 181: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

158

Rahtu, A.;Gordon, R. G. Nat. Mater. 2003, 2, 749, (d) Lim, B. S.; Rahtu, A.; Park, J.

S.; Gordon, R. G. Inorg. Chem. 2003, 42, 7951.

5 Coyle, J. P.; Monillas, W. H.; Yap, G. P. A.; Barry, S. T. Inorg. Chem. 2008, 47,

683.

6 Park, J. W.; Jang, H. S.; Kim, M.; Sung, K.; Lee, S. S.; Chung, T.; Koo, S.; Kim, C.

G.; Kim, Y. Inorg. Chem. Commun. 2004, 7, 463.

7 Grushin, V. V.; Marshall, W. J. Adv. Synth. Catal. 2004, 346, 1457.

8 Knoops, H. C. M.; Langereisb, E.; van de Sandenb, M. C. M.; Kessels, W. M. M J.

Electrochem. Soc. 2010, 157, 12, G241.

9 Gambarotta, S.; Bracci, M.; Floriani, C.; Chiesi-Villa, A.; Guastini, C. J. Chem. Soc.,

Dalton Trans. 1987, 1883.

10 Tsuda, T.; Watanabe, K.; Miyata, K.; Yamamoto, H.; Saegusa, T. Inorg. Chem.

1981, 20, 2728.

11 Gaillard, S.; Cazin, C. J.; Nolan, S. P. Acc. Chem. Res. 2012, 45, 778, and references

therein.

12 (a) Goj, L. A.; Blue, E. D.; Delp, S. A.; Gunnoe, T. B.; Cundar, T. R.; Pierpont, A.

W.; Petersen, J. L.; Boyle, P. D. Inorg. Chem. 2006, 45, 9032, (b) Goj, L. A.; Blue,

E. D.; Munro-Leighton, C.; Gunnoe, T. B.; Petersen , J. L. Inorg. Chem. 2005, 44,

8647.

13 Mankad, N. P.; Laitar, D. S.; Sadighi, J. P. Organometallics 2004, 23, 3369.

14 (a) Niskanen, A.; Hatanpää, T.; Arstila, K.; Leskelä, M.; Ritala, M. Chem. Vap.

Deposition 2007, 13, 408, (b) Kariniemi, M.; Niinistö, J.; Hatanpää, T.; Kemell, M.;

Sajavaara, T.; Ritala, M.; Leskelä, L. Chem. Mater. 2011, 23, 2901

15 Denk, M. K.; Thadani, A.; Hantano, K.; Lough, A. J. Angew. Chem. Int. Ed. 1997,

36, 2607

16 Jain, A.; Chi, K. -M.; Kodas, T. T.; Hampden-Smith, M. J. J. Electronchem. Soc.

1993, 140, 1434

17 (a) Nyburg, S. C.; Parkins, A. W.; Sidi-BouMedine, M. Polyhedron 1993, 12, 1119,

(b) Melzer, M. M.; Mossin, S.; Day, X.; Bartell, A. M.; Kapoor, P.; Meyer, K.;

Warren, T. H. Angew. Chem. Int. Ed. 2010, 49, 904, (c) Harkins, S. B.; Mankad, N.

P.; Miller, A. J. M.; Szilagyi, R. K.; Peters, J. C. J. Am.Chem. Soc. 2008, 130, 3478.

Page 182: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

159

18 James, A. M.; Laxman, R. K.; Fronczek, F. R.; Maverick, A. W. Inorg. Chem. 1998,

37, 3785

19 Elliott, S. D. Semicond. Sci. Tech. 2012, 27, 074008.

20 Widjaja, Y; Musgrave, C. B J. Chem. Phys. 2002, 117, 1931.

21 Jeloaica, L.; Esteve, A.; Rouhani, M. D.; Esteve, D. Appl. Phys. Lett. 2003, 83, 542.

22 Li, J.; Wu, J.; Zhou, C.; Han, B.; Lei, X.; Gordon, R.; Cheng, H. Int. J. Quantum

Chem. 2009, 109, 756.

23 Kwon, J.; Saly, M.; Halls, M. D.; Kanjolia, R. K.; Chabal, Y. J. Chem. Mater. 2012,

24, 1025.

24 (a) Mårtensson, P.; Larsson, K.; Carlsson, J.-O. Appl. Surf. Sci. 1998, 136, 137, (b)

Mårtensson, P.; Larsson, K.; Carlsson, J.-O. Applied Surface Science 1999, 148, 9,

(c) Mårtensson, P.; Larsson, K.; Carlsson, J.-O. Appl. Surf. Sci. 2000, 157, 92.

25 Dai, M.; Kwon, J.; Halls, M. D.; Gordon, R. G.; Chabal, Y. J. Langmuir 2010, 26,

3911.

26 Orimoto, Y.; Toyota, A.; Furuya, T.; Nakamura, H.; Uehara, M.; Yamashita, K.;

Maeda, H. Ind. Eng. Chem. Res. 2009, 48, 3389.

27 Machado, E.; Kaczmarski, M.; Ordejón, P.; Garg, D.; Norman, J.; Cheng, H.

Langmuir 2005, 21, 7608.

28 Dey, G.; Elliott, S. D. J. Phys. Chem. A 2012, 116, 8893.

29 Lee, B. H.; Hwang, J. K.; Nam, J. W.; Lee, S. U.; Kim, J. T.; Koo, S.-M.;

Baunemann, A.; Fischer, R. A.; Sung, M. M. Angew. Chem. Int. Ed. 2009, 48, 4536.

30 a) Lin, J. C. Y.; Huang, R. T. W.; Lee, C. S.; Bhattacharyya, A.; Hwang, W. S.; Lin,

I. J. B. Chem. Rev. 2009, 109, 3561, b) An, D.; Wang, J.; Dong, T.; Yang, Y.; Wen,

T.; Zhu, H.; Lu, X.; Wang, Y. Eur. J. Inorg. Chem. 2010, 4506

31 Kunte, G. V.; Shivashankar, S. A.; Umarji, A. M. Meas. Sci. Technol. 2008, 19,

025704.

32 The 1 Torr values for 1 and 2 are corrected from our previous publication (Coyle et

al. Chem. Mater. 2013, 25, 1132) because of a calculation error for the value of the

sample pan surface area.

Page 183: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

160

33 Park, K.-M.; Kim, J.-K.; Han, B.; Lee, W.-J.; Kim, J.; Shin , H.-K. Microelectron.

Eng. 2012, 89, 27.

34 Niskanen, A.; Rahtu, A; Sajavaara, T.; Arstila, K.; Ritala, M.; Leskela, M. J.

Electrochem. Soc. 2005, 152, G25.

35 Li, Z.; Rahtu, A.; Gordon, R. G. J. Electrochem Soc. 2006, 153, C787

36 Lundqvist, B. I.; Andersson, Y.; Shao, H.; Chan, S.; Langreth, D. C. Int. J. Quantum

Chem. 1995, 56, 247.

37 Ruiz, V. G.; Liu, W.; Zojer, E.; Scheffler, M.; Tkatchenko, A. Phys. Rev. Lett. 2012,

108, 146103.

38 Marom, N.; Tkatchenko, A.; Rossi, M.; Gobre, V. V.; Hod, O.; Scheffler, M.;

Kronik, L. J. Chem. Theory Comput. 2011, 7, 3944.

39 Dubinina, G.G.; Furutachi, H.; Vicic, D. A. J. Am. Chem. Soc. 2008, 130, 8600.

40 Díez-Gonzáez, S.; Escudero-Adán, E. C.; Benet-Buchholz, J.; Stevens, E. D.;

Slawin, A. M. Z.; Nolan, S. P. Dalt. Trans. 2010, 39, 7595.

41 Kuhn, N.; Kratz, T. Synthesis 1993, 561.

42 Bittermann, A.; Baskakov, D.; Herrmann, W. A. Organometallics 2009, 28, 5107.

43 Lappert, M. F.; Slade, M. J.; Singh A.; Atwood, J. L.; Rogers, R. D.; Shakir, R. J.

Am. Chem. Soc. 1983, 105, 302.

44 Schafer, A.; Huber, C.; Ahlrichs, R. J. Chem. Phys. 1994, 100, 5829.

45 Ahlrichs, R.; Bär, M.; Häser, M.; Horn, H.; Kölmel, C. Chem. Phys. Lett. 1989, 162,

165.

46 Perdew, J. P.; Burke, K.; Ernzerhof, M. Phys. Rev. Lett. 1996, 77, 3865.

47 Eichkorn, K.; Weigend, F.; Treutler, O.; Ahlrichs, R. Theor. Chim. Acta. 1997, 97,

119.

48 Sierka, M.; Hogekamp, A.; Ahlrichs, R. J. Chem. Phys. 2003, 118, 9136.

49 Schafer, A.; Horn, H.; Ahlrichs, R. J. Chem. Phys. 1992, 97, 2571.

50 Cioslowski, J. J. Am. Chem. Soc. 1989, 111, 8333.

Page 184: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

161

51 Sheldrick, G.M. Acta Cryst.2008, A64, 112-122.

Page 185: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

162

Synthesis and Thermal Gravimetric Studies of Monomeric 7 Chapter:

Cu(I)N(SiMe3)2 Complexes Supported by N-Heterocyclic and Acyclic

Diamino Carbenes.

A manuscript for the following work is in preparation. Co-contributors to this work

include Eric R. Sirianni1, Ilia Korobkov

2, Glenn P.A. Yap

1, Seán T. Barry

3.

1 Department of Chemistry & Biochemistry, University of Delaware, Newark, Delaware

19716, United States 2 Department of Chemistry, University of Ottawa, Ottawa, K1N 6N5, Canada

3 Department of Chemistry, Carleton University, 1125 Colonel By Drive, Ottawa, K1S

5B6, Canada

Abstract 7.1

Thermal properties of a series of monomeric copper(I) hexamethyldisilazide

complexes supported by N-heterocyclic and acyclic diamino carbenes were evaluated for

consideration as ALD precursors. Ten NHCs and ADCs were selected to study the impact

of N-alkyl substituent and backbone character on volatility and thermal stability. The

series of complexes had melting points of 45 – 184 °C while several complexes were

liquids. Vaporizations rates were measured by stepped-isothermal TGA experiments

between 110 – 170 °C. Enthalpies of vaporization were determined to be 63 – 90 kJ/mol.

Temperatures for 1 Torr of vapor pressure were estimated to be 143 – 172 °C showing a

general dependence on molecular weight. The imidazolylidene complexes were thermally

unstable with strong evidence indicating the unsaturated backbone as a point of

weakness. The imidazolinylidene complexes showed excellent thermal stability with

comparable results for the formamidinylidenes complexes. The steric parameter of the

carbene, %VBur, was calculated for all complexes characterized by single crystal X-ray

diffraction. NHCs and ADCs are suitable additions to the library of ligands available to

precursor design for ALD.

Page 186: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

163

Introduction 7.2

Copper precursors for atomic layer deposition (ALD) and chemical vapour

deposition (CVD) remain a subject of research internationally due to the importance of

copper as an interconnect material in microelectronics.1 Copper is easily reduced to a

metallic film, and this has led to an abundance of copper precursors, including β-

diketonates,2 β-diketiminates,

3 amidinates,

4 guanidinates,

5 aminoalkoxides,

6

pyrrolylaldiminates,7 and disilylamides

8 to name a few.

Three main criteria outline the design of a copper precursor capable of meeting

the requirements for industrial application. These criteria centre on the precursor’s

volatility, thin film deposition chemistry, and chemical composition. The first two criteria

are temperature dependent preferably met at low temperatures to reduce potential issues

related to thermal stability and thin film morphology. The precursor needs to generate

sufficient vapour pressure at a temperature where negligible decomposition or molecular

rearrangement occurs. Precursor chemisorption and reactivity of the surface species to

copper metal at appreciable surface coverages will enable an acceptable growth rate.

Lastly, the precursor molecule must not contain atoms that contaminate or degrade the

barrier and adhesion layers, increase the resistance of the copper interconnect, or

compromise the longevity of the microelectronic devices.

Recently, our efforts have been focused on N-heterocyclic carbenes (NHC)

supported copper(I) amide compounds as volatile precursors for ALD. The typical

copper(I) amide is a tetramer,9 but 1,3-diisopropyl-imidazolin-2-ylidene copper

hexamethyldisilazide (HMDS) was successful employed as a plasma enhanced atomic

layer deposition precursor.1 This compound was shown to have good volatility and

Page 187: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

164

excellent thermal stability over a long time and temperature range. A growth rate for

copper metal at 225 °C of 0.2 Å/cycle was achieved. Interestingly, the similar compound

4,5-dimethyl-1,3-diisopropyl-imidazol-2-ylidene copper HMDS was found to leave a

high residual mass in thermal gravimetric analysis. The main structural difference

between these two compounds was the existence of a double bond in the backbone of the

carbene moiety (Figure 7.1).

Figure 7.1 Structural differences between 1,3-diisopropyl-imidazolin-2-ylidene copper

hexamethyldisilazide (5) and 4,5-dimethyl-1,3-diisopropyl-imidazol-2-ylidene copper

hexamethyldisilazide (3).

As a concept for a copper precursor, the formulation of a NHC copper(I) amide

matches well with the criteria mentioned above. The tendency of NHCs to form linear,

monomeric complexes with copper ensures a low molecular mass to aid volatility. The

high basicity of a metal amide bond can engender surface species amenable to reaction

with reducing agents. Common contaminates, such as halides and oxygen, are avoided.

The variable structural features of NHCs (N-substituents, backbone, and ring size) allows

for tuneable physical characteristics such as thermal stability and volatility. Although, the

strong copper-NHC bond may present a potential drawback as it could hamper precursor

chemisorption.8,10

N-heterocyclic carbenes have risen to become workhorse ligands in

organometallic catalysis.11

Research efforts have mainly focused on the stereo-electronic

Page 188: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

165

effects of the metal-NHC bond to tune catalyst performance with high turnover rates for a

multitude of transformations.12

Decomposition routes of NHC metal complexes13

are also

important to understand in order to circumvent catalyst deactivation.14

Copper NHC

complexes are extremely well studied15

and exploited in catalysis.16

The copper-NHC

bond is very strong (~290 kJ/mol)8,17

and these catalysts have not shown a high

susceptibility to decomposition; therefore, screening of copper NHC catalyst systems

have been performed to optimize catalytic activity18

and not stability.

This encouraged us to explore the effect of the structure of the carbene on the

principle precursor characteristics of these types of compounds. In general, a wide variety

of NHCs can be synthesized.19

We undertook to study the effects of steric bulk on the

nitrogen atoms and at the backbone carbons, as well as the bond order of the carbon-

carbon backbone bond. From the excellent work of Alder et al.,20

acyclic diamino

carbenes (ADC) are also accessible, and this broadened the scope of this study.

Herein we report a series of heterocyclic and acyclic carbenes supporting

copper(I) HMDS. The synthesis, structures, and thermal chemistries are compared across

this family of copper compounds to highlight their potential utility as vapour precursors

for CVD and ALD.

Results and Discussion 7.3

A straightforward approach was used to synthesize the NHC and ADC copper(I)

HMDS complexes. The target complexes were generated by adding 2 equivalents of

lithiated HMDS to solutions of the respective carbene salt and copper chloride in THF

(Figure 7.2). 21

Non-nucleophilic lithium amides are suitable bases to generate free

carbenes19, 20a

and prior isolation of the carbene copper chlorides was unnecessary to

Page 189: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

166

achieve satisfactory yields. Most complexes were sublimed or distilled above 75 °C

under reduced pressure (< 35 mTorr) in fair to very good yields, except for 1 which

decomposed when heated. The procedure for obtaining compound 10 was slightly

modified due to a mixture of counterions in the formamidinium salt.20c

These colourless

compounds quickly turned brown when exposed to air. There are some reports of NHC-

copper complexes reacting readily with O2 to produce the corresponding ketone22

while

free NHCs are sensitive towards H2O.22b

Additionally, [CuN(SiMe3)2]4 decomposes

slowly in air.23

Compounds 8 -10 are the first reported examples of ADC copper

complexes.

Figure 7.2 General Synthetic Conditions for 1-10.

All imidazolium, imidazolinium, formamidinium chlorides were prepared from

known literature methods with the exception of 4,5-dimethyl-1,3-ditertbutyl-

imidazolinium chloride. This new imidazolinium was developed from known synthetic

methods (Figure 7.3). Briefly, a condensation reaction between formaldehyde and

Page 190: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

167

Figure 7.3 Synthesis of 4,5-dimethyl-1,3-ditertbutyl-imidazolinium chloride.

rac-N,N’-di-tert-butyl-2,3-dimethylethylenediamine24

generated the corresponding

aminal which was oxidized by N-chlorosuccinimide.25

Attempts involving the traditional

orthoformate route failed presumably due to steric crowding preventing imidazolinium

salt formation.

Table 7.1 Properties of Diamino Carbene Cu(I) HMDS Compounds 1 – 10.

Compound TGA

residue

(%)a

13CNHC

(ppm)b

13CNHC-

Cu

(ppm)

Δ13

C

(ppm) %Vbur

c Mp

(°C)

1 Torr

@T(°C)

ΔHvap

(kJ/mol) 1 - 210.5 176.9 33.6 - - - -

2 14.7 213.2 177.0 36.2 41.5 119 - -

3 4.4 206.8 173.2 33.6 40 115 158 71.3

4 1.5 237.7 201.3 36.4 - liquid 153 66.1

5 1.1 236.8 200.4 36.4 35.7 51 149 66.5

6 0.7 238.2 201.5 36.7 - 98 172 63.0

7 1.0 238.6 198.3 40.3 42.3 118 162 66.4

8 1.6 259.7 214.1 45.6 30.7 45 143 65.5

9 0.6 252.0 211.4 40.6 - liquid 145 70.5

10 1.1 255.5 221.0 34.6 45.6 184 169 89.6

a TG experiments were preformed with a heating rate of 10 °C/min. Sample masses were

1.3μmol (4 - 6 mg). Residual mass recorded at 350 °C. b 13

C chemical shifts for C2 of the free diamino carbenes were taken from Ref. 28(a)

except for 7 which is reported here.26

c %VBur calculated with scaled (by 1.17) Bondi radii, sphere radius R = 3.5 Å, and

diamino carbene – metal bond length of 2.00 Å.

Page 191: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

168

1H NMR analysis of 1-10 displayed a single set of peaks consistent with the

expectation for a single solution species. The singlet peak for HMDS in 1 – 10 was found

between 0.54 – 0.62 ppm. In [CuN(SiMe3)2]4, this peak was reported at 0.505 ppm.27

For

8 – 10, a single set of peaks for the ADC alkyl groups were observed showing free

rotation around the central C-N bonds. 13

C NMR spectra were also simple to interpret.

The 13

C carbenic (C2) peaks were found within the ranges of 173– 177 ppm for the

imidazolylidenes (1 – 3), 198– 201 ppm for the imidazolinylidenes (4 – 7), and 211– 221

ppm for the formamidinylidenes (8 – 10) (Table 7.1) which is consistent with further

downfield shifts for the stronger σ-donor diamino carbenes.28

Interestingly, the C2 chemical shifts for the free imidazolylidenes in 1 - 3 were

shifted upfield 34 - 36 ppm upon complexation. Similarly, an upfield shift of 36 - 40 ppm

was observed for the imidazolinylidenes in 4 - 7. The upfield shifts for the

formamidinylidenes varied. Compounds 8 and 9 displayed large upfield shifts of 45.6

ppm and 40.5 ppm, respectively, while an upfield shift of only 34 ppm was observed in

10. This trend in upfield shifts coincides with the σ-donor and π-acceptor abilities of the

diamino carbenes.29

Intuitively, this trend can be linked to the π-acceptor property of the

carbene as π-back donation from the copper center would increase the shielding around

C2. π –back bonding from group 11 metals to NHCs is no longer considered as

negligible.17,30

In fact, π-back-bonding has been studied in a series of tripodal NHC group

11 complexes31

and the effects of this phenomenon have manifested in gold catalysis.32

The outlier data point from 10 is possibly due to steric hindrance preventing appropriate

orbital overlap for sufficient π -back-bonding to occur. A more rigorous theoretical and

Page 192: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

169

structural analysis is warranted to fully understand this apparent trend in 13

C chemical

shifts.28a

Figure 7.4 Molecular diagram of 7 (left) and 8 (right) with thermal ellipsoids at 30%

probability. H-atoms omitted for clarity.

Crystals were isolated for several of the compounds (2, 7, 8, and 10) and these

structures were very similar regardless of alkyl groups and indeed regardless of whether

the carbene was heterocyclic or acyclic (Figure 7.4; Table 7.2 & 7.3 in Supporting

Information). In general, the structures deviated only slightly from our previously

reported copper carbene compounds (3 and 5).8

All of the compounds have a roughly linear coordination of copper (~174° -

180°), with 8 showing the highest deviation from linear. This is interesting, since 8 has

the least constraint of the carbene groups, but does not show as high steric bulk as 10

does. This deviation also does not appear to corroborate with the torsion of the

hexamethyldisilazido ligand to the carbene (i.e. N – C – N – Si), which rules out hyper-

conjugation through the copper as having a primary effect on the coordination geometry.

Both the copper carbene bonds (1.87Å – 1.91Å) and the copper amide bonds (1.84Å –

1.87Å) are in a close range across this family of compounds. The Si – N – Si bond angles

Page 193: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

170

range between 126–131°. This bond angle is 117.9° in [CuN(SiMe3)2]4.23

This difference

likely indicates the amido ligand geometry is relaxed from steric pressure in a monomeric

compound.

One interesting aspect of these structures is the angle between the ligand planes.

In all cases, the carbenes were trigonal planar around the carbenic carbon, and in general

the HMDS was trigonal planar around the nitrogen (with 3 showing the largest deviation

at 356°). Most of the compounds had an angle between planes of 74° – 88° (including the

previously reported compound 38), while 5 showed only 56° angle and 8 showed 23°.

This is obviously an effect of steric bulk (and possibly crystalline packing) since these are

the two examples of lower steric bulk carbenes for heterocyclic and acyclic respectively.

Table 7.2 Selected Bond Lenghts and Bond Angles for the Structures of 2, 3, 5, 7, 8 and

10. aData was previously reported and provided for convenience.

8

2 3a 5

a 7 8 10

selected bond lengths (Å)

Cu–C1 1.894(2) 1.881(2) 1.870(5) 1.897(2) 1.905(1) 1.908(1)

Cu–N3 1.864(1) 1.870(2) 1.836(4) 1.870(2) 1.856(1) 1.873(1)

C1–N1 1.369(3) 1.360(3) 1.330(7) 1.343(3) 1.352(2) 1.355(1)

C1–N2 1.362(2) 1.365(3) 1.336(6) 1.354(3) 1.336(2) 1.355(1)

N3–Si1 1.698(2) 1.697(2) 1.680(6) 1.695(2) 1.700(1) 1.662(4)

N3–Si2 1.705(2) 1.692(2) 1.701(5) 1.702(2) 1.704(1) 1.708(4)

selected bond angles (deg)

C1–Cu–N3 179.07(7) 178.59(9) 179.2(2) 175.8(1) 173.78(5) 180.0

N1–C1–N2 104.2(1) 103.8(2) 106.6(5) 108.0(2) 118.6(1) 116.95(18

) Si1–N3–Si2 125.86(9) 131.3(1) 128.2(3) 127.1(1) 126.10(6) 127.45(7)

sum of angles (deg)

N1 360.0 360.0 360.0 359.3 359.1 358.2

N2 360.0 359.9 359.9 359.7 358.8 360.0

N3 357.6 355.7 360.0 359.4 358.6 360.0

C1 360.0 360.0 360.0 359.9 359.7 359.9

angle between planes (deg)

(Si1,N3,Si2)

(N1,C1,N2) 73.9 82.4 56.6 87.9 21.5 82.9

torsion angles (deg)

N1–C1–N3–Si1 82.5(2) 88.4(2) 55.9(5) 85.4(2) 33.4(1) 80.3(9)

N1–C2–C3–N2 0.2(2) 0.8(3) 8.5(7) 28.7(2) - -

Page 194: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

171

The percentage of buried volume (%VBur) is a steric parameter model that

calculates the percentage of a sphere around a metal atom occupied by a ligand.33

This

model can be used for a variety of ligands and has been used extensively in the

characterisation of metal-NHC complexes. The %VBur values were calculated from

experimental structure data and were between 30.7 and 45.6 % (Table 7.1). ItBu2Me2 is a

new NHC with a value of 40.7 %. The series of NHCs in 2, 3, and 7 displays excellent

fine tuning of the steric parameter. The ADC, AMe4, had a value of 30.7 % which is a

higher value than some larger NHCs34

and is likely because of the difference in their core

N-C-N bond angles.

Figure 7.5 Imidazolylidenes and Imidazolinylidenes, N-heterocyclic Carbenes (NHC);

and the Formamidinylidenes, Acyclic Diamino Carbenes (ADC), Evaluated in

Monomeric Cu(I) HMDS Complexes 1-10.

All the carbenes employed in this study (Figure 7.5) were systematically selected

concurrent with thermal gravimetric analysis (TGA) of the corresponding copper

complex. The thermal stability of each complex influenced the subsequent choice of

Page 195: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

172

carbene. Our starting point was IiPr2 simply because imidazolylidenes and

iPr substituents

are ubiquitous in their respective fields of NHCs and CVD precursors. Fittingly, 1 proved

to be the least thermally stable. All attempts to purify 1 by vacuum techniques resulted in

a low yield of viscous oil which contained 1 amongst decomposition products, as

determined by 1H NMR. Decomposition was thwarted by increasing the steric bulk of the

carbene, hence 2 was easily purified in high yields by sublimation. Interestingly, TGA of

2 showed a two feature weight loss curve indicative of decomposition (Figure 7.6).

Figure 7.6 Thermal gravimetric analysis of 2, 3, 5, and 9. Experiments were run under 1

atm nitrogen with a ramp rate of 10 °C/min. Sample sizes were between 5 – 7mg.

Page 196: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

173

An isothermal TGA of 2 at 110 °C showed the first mass loss feature to plateau at

about 60 % residual mass (Figure 7.10 in Supporting Information). The NHC and HMDS

moieties account for 45 % and 40 % of the total mass, respectively. 1H and

13C NMR

analysis in CDCl3 of the residual material found peaks with chemical shifts matching

exactly those for [ItBu2]CuCl.

35 No remnant peaks for HMDS were observed. The

protons residing in the unsaturated backbone of imidazolylidenes are known to be acidic.

They are capable of undergoing deuterium exchange,36

silylation,37

and metalation

affording an anionic N-heterocyclic dicarbene (NHDC).38

Our proposed decomposition

route for 2 is via deprotonation of the unsaturated backbone and elimination of

hexamethyldisilazane forming an anionic NHDC species (Figure 7.7). The [ItBu2]CuCl

species which was identified during NMR analysis likely formed due to HCl in the

CDCl3 and verifies that the N-alkyl substituents of ItBu2 were intact.

Figure 7.7 Thermal Decomposition of [I

tBu2]Cu(I)HMDS (2) via Deportonation of the

Unsaturated NHC Backbone and Elimination of Hexamethyldisilazane.

An NHC with a methylated unsaturated backbone such as in IiPr2Me2 would

prevent this type of decomposition. Compound 3 sublimed in excellent yield and

displayed a single weight loss feature (indicative of volatilization) and a low residual

mass of 4.3 % in a TG experiment (Figure 7.6). The trend in thermal stability of the series

1 – 3 supports our purposed decomposition pathway for 2 and demonstrates how this

Page 197: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

174

thermal reactivity can be kinetically avoided by increasing the steric bulk of the N-alkyl

groups or prevented by methylation of the backbone.

In light of the vulnerability of the unsaturated NHCs, several imidazolinylidenes

were studied in 4 – 7. NHCs with saturated backbones resulted in volatile compounds

with excellent thermal stability. A comparison of the residual masses from TG

experiments of 3 (4.3%) to 5 (1.0 %) (Figure 7.6) highlights the superior thermal stability

of the imidazolinylidenes versus imidazolylidenes. Thermal rearrangements for IiPr2Me2

and ItBu2 occurring through a C-N bond activation have been shown for transition metal

complexes.39

To our knowledge, similar chemistry has not been demonstrated for

imidazolinylidenes which possibly explains their increased stability. The alkyl

substituents for the series of 4 – 7 were chosen in order to study the effect of steric bulk

on thermal stability. The residual masses for these compounds were similar and found

between 0.7 – 1.5 % (Figure 7.11 in Supporting Information).

The contrasting thermal stabilities between the unsaturated and saturated NHC

compounds prompted the selection of ADCs to explore whether the backbone could be

removed while maintaining desirable characteristics of an ALD precursor. TG

experiments of 8 – 10 yielded low residual masses between 0.4 – 1.6 % (Figure 7.12 in

Supporting Information) which demonstrates thermal stability and volatility. The cyclic

nature was thus determined to be an elective feature for the diamino carbene in the design

of these precursors.

Further thermal characterisation of the volatile compounds (3 – 10) was

accomplished by a thermal stress test using the TGA. This test simply varied the sample

mass over several experiments with a constant heating rate. Consequently, the larger

Page 198: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

175

samples are exposed to higher temperatures and more extensive decomposition can occur.

Evidently, evaporation rates play a role and the more volatile compounds have a slight

advantage because lower temperatures are achieved within the window of evaporation.

The thermal stress test is relatively quick to perform compared to other solution based

quantitative methods and generates similar qualitative trends.40

Different molar amounts

were heated at 10 °C/min and the residual mass was converted to a percentage of

decomposition assuming that the residual material was entirely copper. Compounds 3 –

10 showed values for percent decomposition between 2 – 8 % at low sample masses and

between 11 – 86 % at high sample masses (Figure 7.8).

Figure 7.8 TGA thermal stress test for 3 – 10. The heating rate was 10 °C/min for each

experiment. The smallest sample sizes were 1.3 μmol (~5 mg) and the largest were 15.9

μmol (~ 60mg).

Page 199: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

176

For compounds 4 – 7, imidazolinylidenes with bulkier N-substituents imparted

more thermal stability to the respective copper complex. A similar trend was observed for

the formamidinylidenes 8 and 9; however, 10 showed more decomposition than 9. This

dependence of thermal stability on steric bulk suggests that dissociation of the carbene-

copper bond is not the first step during decomposition. Hillier et al. reported that bond

dissociation enthalphies are less for sterically demanding NHCs in the Cp*Ru(NHC)Cl

system.41

Steric bulk within these copper complexes may be preventing oligomerization,

intermolecular disproportionation or possibly a β-methyl42

or γ-H abstraction43

of the

hexamethyldisilazide ligand.

The thermal stress test for 10 was strikingly different compared to the others (Figure 7.13

in Supporting Information). Two distinct weight loss features were observed and the

inflection point appeared at a higher weight percent for higher sample mass loading. The

steric bulk of AiPr4 may be a tipping point for the dissociation of the carbene copper

bond. During the temperature of the experiment the rate of Cu–AiPr4 bond dissociation

would accelerate. Therefore, when large amounts of 10 are exposed to high temperatures

larger amounts of uncoordinated copper amide would remain in the sample pan.

Furthermore, free44

and coordinated28d

AiPr4 have been found to rearrange to

formamidine via propene elimination which would result in a similar outcome as bond

dissociation.

Compound 5 was reported as an ALD precursor with excellent thermal stability

over two weeks when heated at 130 °C. The thermal stress test via TGA showed

compounds 6, 7 and 9 to behave as well or better than 5 and predicts these compounds to

be ideal precursors for ALD.

Page 200: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

177

Stepped isothermal TGA experiments were performed to determine and compare

rates of evaporation. These experiments were performed for compounds 3 – 10 which

were thermally stable within a suitable temperature range (110 – 170°C) and time frame

of the experiment. The results show a general trend where compounds of lower molecular

mass show higher rates of evaporation (Figure 7.9). Interestingly, 7 showed higher rates

of evaporation than 6 even though 7 is higher in mass by two methyl groups. A similar

reversal is evident for 4 and 5, which also differ by two methyl groups. A likely

explanation is that intermolecular van der Waal interactions are disrupted by the addition

of methyl groups. This explanation is counterintuitive since increasing the number of

alkyl groups would likely increase the number of van der Waal interactions.45

However,

the placement of the methyl groups in 5 and 7 are onto methylene carbons adjacent to

unobstructed methylene or methyl carbons. Branching at these particular carbons

prevents a chain of intermolecular interactions and would lower the overall number of

interactions available between two molecules. The higher rates of evaporation for 5 and 7

highlight how judicious alkyl groups can be added to increase evaporation rates.

Page 201: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

178

Figure 7.9 Isothermal rates of vaporization for 3 – 10 under 1 atm of nitrogen.

Vapour pressure data was calculated from the data shown in Figure 7.9 by using

the Langmuir equation.46

The Langmuir equation provides an equality between the rate of

mass loss of a substance and its vapour pressure in a vacuum. To account for the flowing

gas environment of the TGA instrument, a calibration constant was determined using

benzoic acid as a standard. The 1 Torr temperatures for 3 -10 were calculated to be

between 143 – 172 °C (Table 7.1).47

By this method, the 1 Torr value for

copper(II)TMHD was 167 °C which is within 3 % of a measured value of 172 °C.48

The vapour pressure curves showed Arrhenius temperature dependence (R2 >

0.99) for all compounds tested. Enthalpies of vapourization (ΔHvap) could be extracted

using the Classius-Clapeyron equation. The ΔHvap values for 3-9 (Table 7.1) varied

Page 202: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

179

slightly and were found between 63 – 72 kJ/mol. Compound 10 yielded a ΔHvap value of

89.6 kJ/mol but an accurate determination was complicated by its concomitant

decomposition. The ΔHvap values for 3-9 compare well with dimeric copper(I)

amidinates (58.4 – 82.4 kJ/mol)4a

and are lower than monomeric copper(II) β-diketonates

(81- 151 kJ/mol).49

The accuracy of ΔHvap measurements were confirmed with

copper(II)TMHD whose sublimation enthalpy was measured to be 103.9 kJ/mol which is

in good agreement to literature values measured by similar methods.48-50

Conclusion 7.4

A series of NHC and ADC copper(I) hexamethyldisilazide complexes were

synthesized and characterized with a focus on their thermal properties. The carbene and

amide ligands were installed onto the metal center via a single step reaction. The

complexes were monomeric in the gas and solid phase validating the role of the carbene.

All compounds were volatile during vacuum sublimation or distillation. Ramped TGA for

3 - 10 displayed a single weight loss feature resulting in low residual masses

demonstrating these compounds to be thermally stable during volatilization.

The thermal stability of the complexes was strongly dependent on the character of

the carbon-carbon carbene backbone. Steric bulk of the N-substituents was also a

significant factor determining the thermal stability of the complexes. The strength of the

carbene-copper bond was verified as it remained intact at elevated temperature (> 175

°C) during TGA. Dissociation of the carbene-copper bond was not suspected to be the

operative step during decomposition at higher temperatures.

There was a striking difference between the thermal stabilities of the

imidazolylidenes complexes compared to those of the imidazolinylidenes. The thermal

Page 203: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

180

stability of a formamidinylidene complex could be equal to either of the aforementioned

NHC complexes depending on the steric bulk of the N-alkyl substituents. The results

presented here will be useful guidelines for the design of other metal precursors

employing diamino carbenes or to areas of organometallic catalysis where thermal

stability is of interest.

Experimental Section 7.5

General Considerations. All manipulations involving the synthesis and handling

of copper(I) compounds were performed in an MBraun Labmaster 130 Drybox under a

nitrogen atmosphere. All reagents were purchased from either Aldrich Chemical Co. or

Alfa Aesar and used as received. Anhydrous tetrahydrofuran and pentane were purchased

from Aldrich Chemical Co. and used as received. The hydrochloride salts of the NHCs

and ADCs were prepared according to literature: IiPr2,

51 I

tBu2,

36 SI

iPr2,

52 SI

tBu2,

53

AMe4,54

AiPr4.

20a Preparation of the hydrochloride salts for AEt4, SI

tBu2Me2, and SIEt2

are provided below. Compound 38 and Et2O·LiN(SiMe3)2

55 were prepared according to

literature.

Physical Measurements. NMR spectra were recorded on a 400 MHz Bruker

AMX spectrometer. NMR spectra were measured in C6D6 and were referenced against

residual protonated solvent. Thermogravimeteric analysis was performed on a TA

Instrument Q50 apparatus located in an MBraun Labmaster 130 Dry box under a nitrogen

atmosphere in platinum crucibles. Evaporation rates were recorded from a stepped-

isotherm TG experiment where isotherms between 110 – 170 °C were maintained for 10

min and sample masses were 20 – 40 mg. Melting points were measured in capillaries

sealed with vacuum grease using a Mel-Temp II apparatus. High resolution mass

Page 204: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

181

spectrometry was performed on a Kratos Concept – Accurate Mass EI at the John L.

Homes Mass Spectrometry Facility at the University of Ottawa.

1,3-diisopropyl-imidazol-2-ylidene copper hexamethyldisilazide (1): 1,3-

diisopropylimidazolium chloride was suspened in 30 mL of THF and CuCl was added.

The suspension was stirred for 1 h during which it cleared to a solution.

Et2O·LiN(SiMe3)2 dissolved in 10 ml of THF was added dropwise and stirring proceeded

for 18 h. Volatiles were stripped off under reduced pressure. The residual material was

taken up in 10 mL of pentane. The insoluble solids were filtered off and washed with 2 x

2 mL of pentane. All pentane fractions were combined and the pentane was stripped off

under vacuum to afford a light yellow liquid (0.582 g, 77.6 %). 1H NMR (400 MHz,

C6D6): δ 0.62 [s, 18H, N(Si(CH3)3)2], δ 0.95 [d, 12H, NCH(CH3)2], δ 4.69 [sept, 2H,

NCH(CH3)2], δ 6.05 [s, 2H, N(CH)2N]. 13

C NMR (100 MHz, C6D6): δ 7.3

[N(Si(CH3)3)2], δ 23.4 [NCH(CH3)2], δ 53.2 [NCH(CH3)2], δ 116.1 [N(CH)2N], δ 176.9

[NCN]. Compound purity was unsatisfactory for elemental analysis.

1,3-ditertbutyl-imidazol-2-ylidene copper hexamethyldisilazide (2): Compound 2

was prepared in an analogous manner as compound 1 substituting: 1,3-ditertbutyl-

imidazolium chloride (0.396 g, 1.83 mmol), CuCl (0.186 g, 1.88 mmol),

Et2O·LiN(SiMe3)2 (0.882 g, 3.65 mmol). Compound 2 was purified by sublimation (95

°C, 20 mtorr) and collected as a colourless solid (0.612 g, 82.9 %). 1H NMR (400 MHz,

C6D6): δ 0.55 [s, 18H, N(Si(CH3)3)2], δ 1.46 [s, 18H, NC(CH3)3], δ 6.33 [s, 2H,

N(CH2)N]. 13

C NMR (100 MHz, C6D6): δ 6.9 [N(Si(CH3)3)2), δ 31.8 (NC(CH3)3], δ 57.6

[NC(CH3)3], δ 115.7 [N(CH2)N], δ 176.8 [NCN] HRMS (EI) m/z calcd for

C17H38N3Si2Cu M+ 403.1900, found 403.1883.

Page 205: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

182

1,3-diethyl-imidazolin-2-ylidene copper hexamethyldisilazide (4): Compound 4

was prepared in an analogous manner as compound 1 substituting: 1,3-diethyl-

imidazolinium chloride (1.067 g, 6.55 mmol), CuCl (0.668 g, 6.75 mmol),

Et2O·LiN(SiMe3)2 (3.161 g, 13.09 mmol). Compound 4 was purified by distillation (158

°C, 20 mtorr) and collected as a colourless liquid (1.780 g, 77.6 %). 1H NMR (400 MHz,

C6D6): δ 0.57 [s, 18H, N(Si(CH3)3)2] , δ 0.76 [t, 6H, NCH2CH3], δ 2.40 [s, 4H,

N(CH2)2N], δ 3.22 [q, 4H, NCH2CH3]. 13

C NMR (100 MHz, C6D6): δ 7.6 [N(Si(CH3)3)2],

δ 14.2 [NCH2CH3], δ 45.2 [N(CH2)2N], δ 47.5 [NCH2CH3], δ 201.6 [NCN] HRMS (EI)

m/z calcd for C13H32N3Si2Cu M+ 349.1431, found 349.1464.

1,3-diisopropyl-imidazolin-2-ylidene copper hexamethyldisilazide (5): Compound

5 was prepared in an analogus manner as compound 1 substituting: 1,3 diisopropyl-

imidazolinium chloride (0.347 g, 1.82 mmol), CuCl (0.186 g, 1.88 mmol),

Et2O·LiN(SiMe3)2 (0.879 g, 3.64 mmol). Compound 5 was purified by sublimation

employing a dry ice cold finger (93 °C, 35 mtorr) and collected as a colourless solid

(0.592 g, 86.0 %); m.p. 49-51 °C. Analytical data matched previously reported data.8 1H

NMR (400 MHz, C6D6): δ 4.46 [sept, 2H, NCH(CH3)2], δ 2.50 [s, 4H, N(CH2)2N], δ 0.81

[d, 12H, NCH(CH3)2], δ 0.54 [s, 18H, N(Si(CH3)3)2]. 13

C NMR (100 MHz, C6D6): δ

200.4 [NCN], δ 51.2 [NCH(CH3)2], δ 41.9 [N(CH2)2N], δ 20.7 [NCH(CH3)2], δ 7.2

[N(Si(CH3)3)2]. HRMS (EI) m/z calcd for C15H36N3Si2Cu M+ 377.1744, found 377.1763.

1, 3-ditertbutyl-imidazolin-2-ylidene copper hexamethyldisilazide (6): Compound

6 was prepared in an analogus manner as compound 1 substituting: 1,3-ditertbutyl-

imidazolinium chloride (0.350 g, 1.60 mmol), CuCl (0.163 g, 1.65 mmol),

Et2O·LiN(SiMe3)2 (0.773 g, 3.20 mmol). Compound 6 was purified by sublimation (91

Page 206: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

183

°C, 20 mtorr) and collected as a colourless solid (0.548 g, 84.3 %); m.p. 96-98 °C. 1H

NMR (400 MHz, C6D6): δ 0.56 [s, 18H, N(Si(CH3)3)2], δ 1.33 [s, 18H, NC(CH3)3], δ 2.59

[s, 4H, N(CH2)2N]. 13

C NMR (100MHz, C6D6): δ 6.9 [N(Si(CH3)3)2], δ 30.8 [NC(CH3)3],

δ 45.2 [N(CH2)2N], δ 55.0 [NC(CH3)3], δ 201.5 [NCN] HRMS (EI) m/z calcd for

C17H40N3Si2Cu M+ 405.2057, found 405.2031.

4, 5-dimethyl-1, 3-ditertbutyl-imidazolin-2-ylidene copper hexamethyldisilazide

(7): Compound 7 was prepared in an analogus manner as compound 1 substituting: 4,5-

dimethyl-1,3-ditertbutyl-imidazolinium chloride (0.425 g, 1.72 mmol), CuCl (0.176 g,

1.78 mmol), Et2O·LiN(SiMe3)2 (0.832 g, 3.45 mmol). Compound 7 was purified by

sublimation (75 °C, 10 mtorr) and collected as a colourless solid (0.555 g, 74.0 %); m.p.

118 °C. 1H NMR (400 MHz, C6D6): δ 0.55 [d, 6H, N(CHCH3)2N], δ 0.57 [s, 18H,

N(Si(CH3)3)2], δ 1.43 [s, 18H, NC(CH3)3], δ 2.77 [q, 2H, N(CHCH3)2N]. 13

C NMR (100

MHz, C6D6): δ 7.2 [N(Si(CH3)3)2], δ 21.0 [N(CHCH3)2N], δ 32.7 [NC(CH3)3], δ 55.2

[NC(CH3)3], δ 62.3 [N(CHCH3)2N], δ 199.0 [NCN] HRMS (EI) m/z calcd for

C19H44N3Si2Cu M+ 433.2370, found 433.2359.

N,N,N’,N’-tetramethylformamidinylidene copper hexamethyldisilazide (8):

Compound 8 was prepared in an analogous manner as compound 1 substituting:

N,N,N’,N’-tetramethylformamidinium chloride (4.21g, 30.8 mmol) suspended in 100 ml

of THF, CuCl (3.15 g, 31.8 mmol), Et2O·LiN(SiMe3)2 (14.90 g, 61.7 mmol) dissolved in

60 mL THF. 30 mL of pentane was used for the extraction and 3 x 10 mL portions of

pentane were used for washing. Compound 8 was purified by sublimation (90 °C, 20

mtorr) and collected as a colourless solid (8.746 g, 87.5 %). 1H NMR (400 MHz, C6D6): δ

0.56 [s, 18H, N(Si(CH3)3)2], δ 2.43 [s, 12H, N(CH3)2]. 13

C NMR (100MHz, C6D6): δ 7.2

Page 207: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

184

[N(Si(CH3)3)2], δ 44.0 [N(CH3)2], δ 214.1 [NCN] HRMS (EI) m/z calcd for

C11H30N3Si2Cu M+ 323.1274, found 323.1271.

N,N,N’,N’-tetraethylformamidinylidene copper hexamethyldisilazide (9):

Compound 9 was prepared in an analogous manner as compound 1 substituting:

N,N,N’,N’-tetraethylformamidinium chloride (0.760 g, 3.94 mmol), CuCl (0.403 g, 4.07

mmol), Et2O·LiN(SiMe3)2 (1.905 g, 7.89 mmol). Compound 9 was purified by distillation

(148 °C, 10 mtorr) and collected as a light yellow liquid (1.010 g, 67.3 %). 1H NMR (400

MHz, C6D6): δ 0.56 [s, 18H, N(Si(CH3)3)2], δ 0.80 [t, 12H, N(CH2CH3)2], δ 3.07 [q, 8H,

N(CH2CH3)2]. 13

C NMR (100 MHz, C6D6): δ 7.6 [N(Si(CH3)3)2], δ 15.2 [N(CH2CH3)2], δ

49.3 [N(CH2CH3)2], δ 211.8 [NCN]. HRMS (EI) m/z calcd for C15H38N3Si2Cu M+

379.1900, found 379.1866.

N,N,N’,N’-tetraisopropylformamidinylidene copper hexamethyldisilazide (10):

N,N,N’,N’-tetraisopropylformamidinium chloride (0.569 g, 2.29 mmol) was suspended in

30 mL of THF and copper(I) chloride (0.233 g, 2.35 mmol) was added. The suspension

was stirred for 18 h. A light pink solid was collected by filtration, washed with 3 x 2 mL

of THF and then dried under vacuum. (This solid was presumed to be of equal ratio of the

formamidinium chloride and copper(I) chloride). The pink solid (0.645 g, 1.85 mmol)

was suspended in 30 mL of toluene and cooled to -35 °C. Et2O·LiN(SiMe3)2 (0.895 g,

3.71 mmol) was dissolved in 20 mL solution of toluene and diethyl ether (1:1) and added

drop wise. The resultant mixture was allowed to warm to room temperature and was

stirred for 18 h. The cloudy solution was filtered and the insoluble fraction was washed

with 2 x 2 mL of toluene. The clear filtrate was combined with the washings and

concentrated under vacuum to 15 mL. The solution was chilled to -35 °C for 4 days to

Page 208: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

185

allow for the crystallization of a colourless solid. The solid was collected by decanting

the solution and was dried under vacuum (0.598 g, 59.9 %). 1H NMR (400 MHz, C6D6):

δ 0.54 [s, 18H, N(Si(CH3)3)2], δ 1.20 [d, 24H, N(CH(CH3)2)2], δ 3.28 [sept, 4H,

N(CH(CH3)2)2]. 13

C NMR (100, MHz, C6D6): δ 6.8 [N(Si(CH3)3)2], δ 24.0

[N(CH(CH3)2)2], δ 51.7 [N(CH(CH3)2)2], δ 220.9 [NCN]. HRMS (EI) m/z calcd for

C19H46N3Si2Cu M+ 435.2526, found 435.2544.

4,5-dimethyl-1,3-ditertbutyl-imidazolinium chloride: Cooled 54 mL of 1.6 M

MeLi in 80 mL of Et2O to 0°C under a N2 atmosphere. N,N’-ditertbutylethylenediimine

(7.28 g, 43.3 mmol) was added in seven portions separated by 10 minutes. The solution

was allowed to warm to RT and stirring proceded for 3 h. The solution was re-cooled to 0

°C and 40 mL of distilled H2O was added dropwise and stirred for 12 h. The organic

layer was decanted and the aqueous layer was extracted with 2 x 40 mL of Et2O. The

organic layers were combined and washed with 20 ml of distilled H2O. Paraformaldehyde

(1.455 g, 48.8 mmol) was added to the Et2O solution and stirred for 24 h. The reaction

solution was dried over MgSO4 and volatiles were removed under reduced pressure to

afford the presummed 4,5-dimethyl-1,3-ditertbutylimidazolidine (8.79 g, 41.4 mmol,

95.7%). 4,5-dimethyl-1,3-ditertbutylimidazolidine (5.000 g, 23.5 mmol) was dissolved in

100 ml of dimethoxyethane and cooled to 0 °C. N-chlorosuccinimide (3.144 g, 23.5

mmol) was added portionwise afterwhich the solution was stirred overnight at RT.

Volatiles were stripped off under reduced pressure and the succinimide by-product was

removed by sublimation (130 °C, 30 mtorr) to afford the crude product as a brown solid

(3.673 g, 63.2 %). 1H NMR (400 MHz, CDCl3): δ 1.38 [d, 6H N(CHCH3)2N], δ 1.61 [s,

18H, NC(CH3)3], δ 3.81 [q, 2H, N(CHCH3)2N], δ 9.54 [s, 1H, NCHN]. 13

C NMR (100

Page 209: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

186

MHz, CDCl3): δ 21.0 [N(CHCH3)2N], δ 30.1 [NC(CH3)3], δ 57.7 [NC(CH3)3], δ 62.9

[N(CHCH3)2N], δ 154.5 [NCHN].

1,3-diethyl-imidazolinium chloride: N,N’-diethylethylenediamine (4.55 g, 39.2

mmol) was dissolved in 100 mL of triethylorthoformate under a nitrogen atmosphere.

The solution was cooled to 0 °C and 4 M HCl in 1,4-dioxane (19.6 mL, 78.3 mmol) was

added dropwise. A volumous white precipitate formed and the reaction mixture was

stirred for 1 h. Two drops of formic acid where added the mixture was refluxed under N2

at 120 °C for 24 h. The clear reaction solution was cooled and 400 mL of heptane was

added to separate the reaction mixture into two layers. The top layer was discarded and

the bottom layer was stripped of volatiles under reduced pressure and dried overnight

under vacuum to afford a light brown solid (4.367 g, 71 %). 1H NMR (400 MHz, CDCl3):

δ 1.36 [t, 6H, NCH2CH3], δ 3.72 [q, 4H, NCH2CH3], δ 4.01 [s, 4H, N(CH2)2N], δ 10.09

[s, 1H, NCHN]. 13

C NMR (100 MHz, CDCl3): δ 13.0 [NCH2CH3], δ 43.1 [NCH2CH3], δ

47.8 [N(CH2)2N], δ 158.0 [NCHN].

N,N,N’,N’-tetraethylformamidinium chloride: N,N-diethylformamide (7.36 mL,

66.1 mmol) and diethylcarbamoyl chloride (23.24 mL, 183.4 mmol) were added to a

pressure vessel and backflushed with N2. The pressure vessel was heated to 145 °C in an

oil bath for 48 h. The pressure vessel was removed from the oil bath. The brown solution

solidified as the pressure vessel cooled to RT. The solid was washed with 3 x 30 mL of

Et2O and dried under vacuum to afford a light brown solid (11.305 g, 75.4 %). 1H NMR

(400 MHz, CDCl3): δ 1.34 [br s, 12H, N(CH2CH3)2], δ 3.48 [br s, 4H, N(CH2CH3)2], δ

3.85 [br s, 4H, N(CH2CH3)2], δ 9.49 [s, 1H, NCHN]. 13

C NMR (100 MHz, CDCl3): δ

Page 210: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

187

14.4 [N(CH2CH3)2], δ 14.7 [N’(CH2CH3)2], δ 43.0 [N(CH2CH3)2], δ 51.6 [N’(CH2CH3)2],

δ 155.8 [NCHN].

Crystallography: Crystallographic studies for 2, 7, 8, and 10: Crystals were

mounted using viscous oil onto a plastic mesh and cooled to the data collection

temperature. Data were collected on a Bruker-AXS APEX CCD diffractometer with

graphite-monochromated Mo-Kα radiation (λ=0.71073 Å). Unit cell parameters were

obtained from 36 data frames, 0.3º ω, from three different sections of the Ewald sphere.

No symmetry higher than triclinic was observed in 2 and 8. The systematic absences in

the diffraction data are consistent with Cc and C2/c for 10 and, uniquely, with P21/n for

7. For 8, and 10, solution in the centrosymmetric space group option yielded chemically

reasonable and computationally stable results of refinement. The data-sets were treated

with absorption corrections based on redundant multiscan data. The structures were

solved using direct methods and refined with full-matrix, least-squares procedures on F2.

To compensate for imprecision introduced by molecular disorder on the crystallographic

two-fold axis, the C-N distances in 10 were constrained to a common yet refined value.

All non-hydrogen atoms were refined with anisotropic displacement parameters. All

hydrogen atoms were treated as idealized contributions. Scattering factors are contained

in several versions of the SHELXTL program library.56

The CIFs have been deposited

under CCDC 1021530 – 1201532 and 1021719.

Page 211: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

188

Supporting Information 7.6

Table 7.3 Crystal Data and Structure Refinement Parameters.

2 7 8 10

formula C17H38CuN3Si2 C19H44CuN3Si2 C11H30CuN3Si2 C19H46CuN3Si2

formula weight 404.23 434.30 324.10 436.31

crystal system triclinic monoclinic triclinic monoclinic

space group P -1 P21/n P -1 C 2/c

a (Å) 8.928(2) 13.876(6) 8.6287(5) 15.3322(5)

b (Å) 9.911(3) 10.287(4) 9.6320(5) 12.6279(4)

c (Å) 14.638(4) 18.863(8) 11.7892(6) 14.4925(5)

α (°) 107.129(4) 90.00 80.207(2) 90.00

β (°) 101.712(4) 106.086(8) 82.472(2) 107.756(1)

γ (°) 101.579(4) 90.00 67.289(2) 90.00

V (Å3) 1164.1(5) 2587.1(18) 888.15(8) 2672.28(15)

Z 2 4 2 4

ρ (g/cm3) 1.153 1.115 1.212 1.084

goodness of fit 1.035 1.007 1.050 1.014

R(Fo) 0.0333 0.0415 0.0204 0.0212

wR(Fo) 0.0935 0.0980 0.0562 0.0556

Page 212: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

189

Figure 7.10 Isothermal TGA experiment of compound 2. An isotherm at 110 °C was

maintained until mass loss was negligible, followed by heating at a rate of 10 °C/min.

Page 213: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

190

Figure 7.11 TGA experiments for the imidazolinylidene Cu(I) HMDS compounds 4 – 7

under 1 atm N2. The heating rate was 10 °C/min and sample masses were 4 – 6 mg.

Page 214: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

191

Figure 7.12 TGA experiments for the formamidinylidene Cu(I) HMDS compounds 8 –

10 under 1 atm N2. The heating rate was 10 °C/min and sample masses were 4 – 6 mg.

Page 215: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

192

Figure 7.13 TGA thermal stress test for compound 10 illustrating thermal decomposition.

The heating rate was 10 °C/min and sample masses are shown top right.

Page 216: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

193

References 7.7

1 International Technology Roadmap for Semiconductors; 2013; http://www.itrs.net/.

2 (a) Chen, T. Y.; Omnes, L.; Vaisserman, J.; Doppelt, P. Inorg. Chim. Acta. 2004,

357, 1299, (b) Bollmann, D.; Merkel, R.; Klumpp, A. Microelectron. Eng. 1997,

37-8, 105, (c) Lagalante, A. F.; Hansen, B. N.; Bruno, T. J.; Sievers, R. E. Inorg.

Chem. 1995, 34, 5781 (d) Wenzel, T. J.; Williams, E. J.; Haltiwanger, R. C.;

Sievers, R. E. Polyhedron 1985, 4, 369.

3 Park, K. H.; Marshall, W. J. J. Am. Chem. Soc. 2005, 127, 9330.

4 (a) Li, Z. W.; Rahtu, A.; Gordon, R. G. J. Electrochem. Soc. 2006, 153, C787, (b)

Li, Z. W.; Barry, S. T.; Gordon, R. G. Inorg. Chem. 2005, 44, 1728, (c) Lim, B. S.;

Rahtu, A.; Gordon, R. G. Nat. Mater. 2003, 2, 749, (d) Lim, B. S.; Rahtu, A.; Park,

J. S.; Gordon, R. G. Inorg. Chem. 2003, 42, 7951.

5 Coyle, J. P.; Monillas, W. H.; Yap, G. P. A.; Barry, S. T. Inorg. Chem. 2008, 47,

683.

6 Park, J. W.; Jang, H. S.; Kim, M.; Sung, K.; Lee, S. S.; Chung, T.; Koo, S.; Kim, C.

G.; Kim, Y. Inorg. Chem. Commun. 2004, 7, 463.

7 Grushin, V. V.; Marshall, W. J. Adv. Synth. Catal. 2004, 346, 1457.

8 Coyle, J. P.; Dey, G.; Sirianni, E. R.; Kemell, M. L.; Yap, G. P. A.; Ritala, M.;

Leskelä, M. Elliot, S. D.; Barry, S. T. Chem. Mater. 2013, 25, 1132.

9 Gambarotta, S.; Bracci, M.; Floriani, C.; Chiesi-Villa, A.; Guastini, C. J. Chem.

Soc. Dalton Trans. 1987, 1883.

10 Dey, G.; Elliott, S. D. Theor. Chem. Acc. 2014, 133, 1416.

11 Hopkinson, M. N.; Richter, C.; Schedler, M.; Glorius, F. Nature 2014, 510, 485.

12 (a) Dröge, T.; Glorius, F. Angew. Chem. Int. Ed. 2010, 49, 6940, (b) Kumar, A.;

Ghosh, P. Eur. J. Inorg. Chem. 2012, 3955.

13 Praetorius, J. M.; Crudden, C. M. RSC Catalysis Series, 2011, 6, 77.

14 Kuhn, K. M.; Bourg, J.-B.; Chung, C. K.; Virgil, S. C.; Grubbs, R. H. J. Am. Chem.

Soc., 2009, 131, 5313.

Page 217: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

194

15 Lin, J. C. Y.; Huang, R. T. W.; Lee, C. S.; Bhattacharyya, A.; Hwang, W. S.; Lin, I.

J. B. Chem. Rev. 2009, 109, 3561.

16 Egbert, J. D.; Cazin, C. S.; Nolan, S. P. Catal. Sci. Technol. 2013, 3, 912.

17 Nemcsok, D.; Wichmann, K.; Frenking, G. Organometallics 2004, 23, 3640.

18 Díez-González, S.; Escudero-Adán, E. C.; Benet-Buchholz, J.; Stevens, E. D.;

Slawin, A. M. Z.; Nolan, S. P. Dalton Trans., 2010, 39, 7595.

19 Hahn, F. E.; Jahnke, M. C. Angew. Chem. Int. Ed. 2008, 47, 3122.

20 (a) Alder, R. W.; Allen, P. R.; Murray, M.; Orpen, A. G. Angew. Chem. Int. Ed.

1996, 35, 1121. (b) Alder, R. W.; Blake, M. E.; Chaker, L.; Harvey, J. N.; Paolini,

F.; Schutz, J. Angew. Chem. Int. Ed. 2004, 43, 5896. (c) Alder, R. W.; Blake, M. E.;

Bufali, S.; Butts, C. P.; Orpen, A. G.; Schütz, J.; Williams, S. J. J. Chem. Soc.,

Perkin Trans. 1. 2001, 1586.

21 The carbene salts and copper chloride are insoluble in THF on their own, but

dissolved when mixed together presumably forming a cuprate ion pair,

[NHC·H+][CuCl2ˉ]. For example: Blue, E. D.; Gunnoe, T. B.; Petersen, J. L.;

Boyle, P. D. J. Organomet. Chem. 2006, 691, 5988 and ref. 22d.

22 (a) Slivarichova, M.; Ahmad, R.; Kuo, Y.-Y.; Nunn, J.; Haddow, M. F.; Othman,

H.; Owen, G. R. Organometallics 2011, 30, 4779. (b) Denk, M. K.; Rodezno, J. M.;

Gupta, S.; Lough, A. J. J. Organomet. Chem. 2001, 617-618, 242 (c) Citadelle. C.

A.; Le Nouy, E.; Bisaro, F.; Slawin, A. M. Z.; Cazin, C. S. J. Dalton Trans. 2010,

39, 4489. (d) Santoro, O.; Collado, A.; Slawin, A. M. Z.; Nolan, S. P.; Cazin, C. S.

J. Chem. Comm.2013, 49, 10483.

23 James, A. M.; Laxman, R. K.; Fronczek, F. R.; Maverick, A. W. Inorg. Chem.

1998, 37, 3785

24 Li W.; Hill, J. N.; Tomasik, A. C.; Bikzhanova, G.; West, R. Organometallics

2006, 25, 3802

25 Mayr, M.; Wurst, K.; Ongania, K.-H.; Buchmeiser, M. R. Chem. Eur. J. 2004, 10,

1256.

26 SItBu2Me2·HCl was treated with 1 equiv. of LiHMDS in THF. SI

tBu2Me2 was

extracted with pentane from the dry reaction solid after removal of volatile

materials in vacuo. 1H NMR (400 MHz, C6D6): δ 0.91 [d, 6H], δ 1.43 [s, 18H], δ

3.07 [q, 2H]. 13

C NMR (100 MHz, C6D6) : δ 22.8, δ 31.8, δ 54.0, δ 62.7, δ 238.6.

Page 218: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

195

27 West, J. K.; Fondong, G. L.; Noll, B. C.; Stahl, L. Dalton Trans. 2013, 42, 3835.

28 (a) Tapu, D.; Dixon, D. A.; Roe, C. Chem. Rev. 2009, 109, 3385. (b) Nelson, D. J.;

Nolan, S. P. Chem. Soc. Rev. 2013, 42, 6723. (c) Huynh, H. V.; Han, Y.; Jothibasu,

R.; Yang, J. A. Organometallics 2009, 28, 5395. (d) Frey, G. D.; Herdtweck, E.;

Herrmann, W. A. J. Organomet. Chem. 2006, 691, 2465

29 Back, O.; Henry-Ellinger, M.; Martin, C. D.; Martin, D.; Bertrand, G. Angew.

Chem. Int. Ed. 2013, 52, 2939.

30 (a) Jacobsen, H.; Correa, A.; Poater, A.; Costabile, C.; Luigi, C. Coord. Chem. Rev.

2009, 253, 687. (b) Marchione, D.; Belpassi, L.; Bistoni, G.; Macchioni, A.;

Tarantelli, F.; Zuccaccia, D. Organometallics 2014, 33, 4200.

31 Hu, X.; Castro-Rodriguez, I.; Olsen, K.; Meyer, K. Organometallics 2004, 23, 755.

32 Alcarazo, M.; Stork, T.; Anoop, A.; Thiel, W.; Fürstner, A. Angew. Chem. Int. Ed.

2010, 49, 2542.

33 Poater, A.; Cosenza, B.; Correa, A.; Giudice, S.; Ragone, F.; Scarano, V.; Cavallo,

L. Eur. J. Inorg. Chem. 2009, 1759.

34 Clavier, H.; Nolan, S. P. Chem. Comm. 2010, 46, 841.

35 1H NMR analysis found two singlets at 1.79 ppm and 7.05 ppm which integrated to

a 1:9 ratio. 13

C NMR analysis found peaks at 32.1 ppm, 57.7 ppm and 116.5 ppm.

These chemical shifts are an exact match to those reported for [ItBu2]CuCl in ref.

18. The residual material from TGA was insoluble in most solvents. It dissolved

slowly in CDCl3 presumably via reaction with residual HCl.

36 Denk, M. K.; Rodezno, J. M. J. Organomet. Chem. 2000, 608, 122.

37 Dubinina, G. G.; Furutachi, H.; Vicic, D. A. J. Am. Soc. Chem. 2008, 130, 8600.

38 Wang, Y.; Xie, Y.; Abraham, M. Y.; Wei, P.; Schaefer, H. F. III; Schleyer, P. v. R.;

Robinson, G. H. J. Am. Soc. Chem. 2010, 132, 14370.

39 (a) Caddick, S.; Cloke, F. G. N.; Hitchcock, P. B.; Lewis, A. K. de, K. Angew.

Chem. Int. Ed. 2004, 43, 5824. (b) Burling, S.; Mahon, M. F.; Powell, R. E.;

Whittlesey, M. K.; Williams, J. M. J. J. Am. Soc. Chem. 2006, 128, 13702. (c) Day,

B. M.; Pugh, T.; Hendriks, D.; Guerra, C. F.; Evans, D. J.; Bickelhaupt, F. M.;

Layfield, R. A. J. Am. Chem. Soc. 2013, 135, 13338.

Page 219: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

196

40 Coyle, J. P.; Pallister, P. J.; Kurek, A.; Sirianni, E. R.; Yap, G. P. A. Barry, S. T.

Inorg. Chem. 2013, 52, 910.

41 Hillier, A. C.; Sommer, W. J.; Yong, B. S.; Petersen, J. L.; Cavallo, L.; Nolan, S. P.

Organometallics 2003, 22, 4322.

42 Yi, W.; Zhang, J.; Chen, Z.; Zhou, X. Inorg. Chem. 2012, 51, 10631.

43 (a) Yu, X.; Bi, S.; Guzei, I. A.; Lin, Z.; Xue, Z.-L. Inorg. Chem. 2004, 43, 7111. (b)

Korobkov, I.; Gambarotta, S. Inorg. Chem. 2010, 49, 3409.

44 Schulz, T.; Leibold, M.; Färber, C.; Maurer, M.; Porsch, T.; Holthausen, M. C.;

Siemeling, U. Chem. Comm. 2012, 48, 9123.

45 Gillan, E. G.; Bott, S. C.; Barron, A. R. Chem. Mater. 1997, 9, 796.

46 Kunte, G. V.; Shivashankar, S. A.; Umarji, A. M. Meas. Sci. Technol. 2008, 19,

025704.

47 The 1 Torr values for 3 and 5 are corrected from our previous publication

(reference 8) because of a calculation error for the value of the sample pan surface

area.

48 Waffenschmidt, E.; Musolf, J.; Heuken, M.; Heime, K. J. Supercond. 1992, 5, 119.

49 Igumenov, I. K.; Basova, T. V.; Belosludov, V. R. Volatile Precursors for Films

Deposition: Vapor Pressure, Structure and Thermodynamics. In Application of

Thermodynamics to Biological and Materials Science, Tadashi, M., Ed.; InTech:

Rijeka, 2011, pp. 521-546.

50 (a) Johnson, M. G.; Selvakumar, J.; Nagaraja, K. S. Thermochimica Acta 2009,

495, 38. (b) Colominas, C.; Lau, K. H.; Hildenbrand, D. L.; Crouch-Baker, S.;

Sanjurjo, A. J. Chem. Eng. Data 2001, 46, 446.

51 Arduengo, A. J., III. U.S., Patent 5182405, 1993.

52 Bittermann, A.; Baskakov, D.; Herrmann, W. A. Organometallics, 2009, 28, 5107.

53 Arentsen, K. Caddick, S. Cloke, F. G. N. Tetrahedron, 2005, 61, 9710.

54 Wasserman, H. H.; Ives, J. L. J. Org. Chem. 1985, 50, 3573.

55 Lappert, M. F.; Slade, M. J.; Singh, A.; Atwood, J. L.; Rogers, D. R.; Shakir, R. J.

Am . Soc. Chem. 1983, 105, 302.

Page 220: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

197

56 Sheldrick, G.M. Acta Cryst.2008, A64, 112-122

Page 221: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

198

Conclusions 8 Chapter:

Two research programs pertaining to the development of precursors for the atomic

layer deposition of copper metal thin films were carried out. Each program set out in a

unique direction while ending, in each case, with new and advanced copper precursors.

The first program built on the well-known copper(I) amidinate precursors. Several

modifications to the amidinate framework were made and the effects on the thermal

chemistry of the respective copper compounds were studied. By this approach,

weaknesses of a ligand framework were identified and ways to prevent thermolysis routes

could be explored. Copper(I) tert-butyl-imino-2,2-dimethylpyrrolidinate was discovered

through this manner and it demonstrates a high level of thermal stability. The second

program was initiated by experiments aimed at breaking the dimeric copper(I) amidinate

structure with N-heterocyclic carbenes. Instead, a popular ligand in organometallic

chemistry was introduced to precursor design and, consequently, the small void of

copper(I) amide complexes in the library of copper ALD precursors was filled. This

particular precursor formulation, i.e. NHC-Cu-NR2, was unknown and required

optimization through a similar process responsible for the advancement of copper(I)

amidinates to iminopyrrolidinates

Both research programs relied extensively on the synthesis of new compounds and

characterisation by thermal gravimetric analysis to validate precursor concepts. Advanced

gas-phase techniques were invaluable in determining between decomposition

mechanisms that were not easily distinguished by bench-top experiments. Much of the

precursor development proceeded without ALD experiments to validate or influence the

design choices. The knowledge gained from this work allowed for many comparisons

Page 222: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

199

between the principle characteristics of the potential precursors, however; it was not

determined if these precursor differences have a substantial effect on the characteristics

of film growth during ALD, e.g. growth rate or ALD temperature window.

Copper(I) guanidinates were synthesized and characterised by thermal gravimetric

analysis, solution decomposition studies and in-situ mass-spectrometry monitoring of

gas-phase thermolysis products during chemical vapour deposition experiments. Results

for the copper(I) guanidinates were compared to a copper(I) amidinate. A latter study

reported two additional copper(I) guanidinates and completed a series of four

compounds, [Cu(iPrN)2CNR’R”]2 where R’ = R” = Me, Et,

iPr and R’ = H, R” =

iPr.

1 The

volatility of the copper(I) guanidinates compared well to that of the copper(I) amidinate.

Noticeable differences were apparent in the geometry of their metallocycles and their

observed decomposition products. Participation of the exocyclic nitrogen in the

guanidinate ligand caused pyramidalization of the chelating nitrogens and twisting of the

metallocycle core of the dimer. The degree of twisting was dictated by the alignment of

the exocyclic lone pair with the delocalized π-system of the ligand which was influenced

by the steric bulk of the exocyclic substituents. Evidence for the production of CDI

during decomposition studies was found for the copper(I) guanidinates and not for the

amidinate. The structural differences could be viewed as influential in the thermoylsis

products since ligand flexibility and acrobatics would be required to deinsert a core

fragment from the guanidinate ligand. Follow-up solution studies for two parent

guanidines, iPr2NC(N

iPr)2H and Me2NC(N

iPr)2H, revealed CDI deinsertion to occur

under similar conditions used for the copper(I) guanidinates.1 Thus it is important to

reconsider the origin of CDI and the possibility of accessible protic species or proton

Page 223: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

200

sources during the solution studies (e.g. dehydrogenation of the ligand, solvent impurities

or the SiO2 surface of NMR tube). Reasonably, it would be worthwhile to revisit the

solution studies with a copper(I) guanidinate containing an exocyclic nitrogen with

substituents that would enable easy identification of the imine produced after CDI

deinsertion, e.g. [Cu(NiPr)2CN

nBu2]2.

CVD experiments for the copper(I) guanidinates demonstrated its utility as a single

source precursor for pure copper metal thin films, similar to copper(I) diketonates

precursors, albeit by a different surface mechanism. Future work for copper(I)

guanidinates should focus on ALD experiments and investigate their temperature window

for self-limited film growth in comparison to the copper(I) amidinates. Particular

attention should be paid to low deposition temperatures, perhaps by PE-ALD, to

determine if the twisted metallocycle assists in chemisorption at lower temperature.

Thermal chemistry for [Cu(NiPr)2CNMe2]2 on a Ni(110) single crystal under ultrahigh

vacuum conditions have been reported, succeeding earlier reports for [CuN(sBu)2CMe]2,

and no evidence was obtained for CDI deinsertion.2

Gas-phase thermolysis products for [Cu(NiPr)2CNMe2]2 were identified TOF MS

and MI FTIR. These advanced techniques were capable of unambiguously identifying

decomposition fragments due to the high resolution and detection limits of the mass

spectrometer combined with the ability to corroborate with highly resolved infrared

spectra. N,N-dimethyl-N’-iso-propyl-N”-iso-propylidene-guanidine, referred to as

oxidized guanidine, was identified as a thermolysis product of [Cu(NiPr)2CNMe2]2 above

150 °C. Deposition of copper inside the thermolysis oven and molecular hydrogen were

also observed. A β-hydride mechanism was proposed and was determined to be operative

Page 224: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

201

up to temperatures of 700 °C in the gas phase. UHV surface studies of

[Cu(NiPr)2CNMe2]2 also identified oxidized guanidine as a product of decomposition.

2

DFT calculations were performed to help rationalize the fact that carbodimide

deinsertion was observed at lower temperatures in the solution phase, but β-hydrogen

elimination is favored in higher temperature, gas phase reactions. DFT calculations at the

B3LYP/6-31+G(d,p) level of theory employing dispersion-correcting potential showed

that at 298 K production of oxidized guanidine (ΔG = -24.4 kcal/mol, Figure 3.5) is

thermodynamically favourable compared to CDI deinsetion (ΔG = -11.7 kcal/mol, Figure

3.1). At 533 K, the two decomposition pathways were equally exergonic, ΔG = -44.4

kcal/mol. Although enthalpy corrections are temperature dependent, the CDI deinsertion

pathway has a more significant entropic driving force. An extensive DFT study modeled

the fragmentation steps for the two pathways through a common intermediate and found

β-hydrogen elimination and CDI deinsertion to be endergonic and exergonic pathways,

respectively. This result helped rationalize why two pathways were discovered

experimentally, but does not clearly explain why only β-hydrogen elimination was

observed in the gas phase experiments. Perhaps, an alternate pathway for β-hydrogen

elimination is possible which provides a low energy detour to the common intermediate.3

Copper(I) iminopyrrolidinates were synthesised to test modifications to the

amidinate ligand designed to block decomposition pathways. Tethering one N-substituent

to the exocyclic position inhibits the CDI deinsertion pathway while replacing β-

hydrogens with methyl groups prevents the β-hydride abstraction pathway. Several

copper(I) iminopyrrolidinates showed lower volatility than [Cu(NiPr)2CNMe2]2. In

solution thermolysis experiments, comparable decompositions rates were measured for

Page 225: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

202

the iminopyrrolidinates compounds possessing β -hydrogens and for [Cu(NiPr)2CNMe2]2

at 165 °C. Copper(I) tert-butyl-imino-2,2-dimethylpyrrolidinate possesses no β-

hydrogens and was stable indefinitely at 165 °C in solution and during TGA.

Copper(I) tert-butyl-imino-2,2-dimethylpyrrolidinate required temperatures

>275°C to chemisorb on high surface area silica which occurred with simultaneous

elimination of its tert-butyl group, presumably as isobutene. Future ALD experiments

exploring its ALD temperature window will complete the list of advantages and

disadvantages for these particular ligand modifications. For instance, due to the rigidity

of the robust iminopyrrolidinate ligand, high temperatures may be necessary to evaporate

and chemisorb the precursor which would be an overall disadvantage compared to other

precursors.

Thermal chemistry for copper(I) N-sec-butyl-iminopyrrolidinate on a Ni(110)

single crystal has been investigated and similar experiments are underway for copper(I)

tert-butyl-imino-2,2-dimethylpyrrolidinate.2 The oxidized iminopyrrolidine, 2-sec-

butyleneamino-1-pyrroline, was observed as a gas phase product at ~300 K, thus β-

hydride abstraction is expected to take place immediately upon precursor adsorption

under film deposition conditions. The transition of adsorbed Cu(I) atoms to Cu(0) was

observed at 350 – 400 K and desorption of smaller dehydrogenated ligand fragments

were observed above 420 K indicating that not all adsorbed iminopyrrolidinate ligand

undergoes β-hydrogen elimination. The remaining surface chemistry for the

iminopyrrolidinate ligand is qualitatively similar to what was previously observed for

[Cu(NsBu)2CMe]2

4 - a core C-N bond breaks and the remaining halves of the ligands

undergo further dehydrogenation chemistry. The main difference for iminopyrrolidinates

Page 226: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

203

is that one half of the ligand is cyclic which implies that susceptible bonds are slightly

constrained from interacting with the surface. Upcoming experiments for copper(I) tert-

butyl-imino-2,2-dimethylpyrrolidinate will tell whether the methylated ring inhibits

surface dehydrogenation reactions and increase the robustness of the adsorbed precursor.

If so, it would be a worthwhile endeavor to explore various copper(I) alkyl-imino-2,2-

dimethylpyrrolidinate precursors to optimize precursor volatility while maintaining

robust surface chemistry.

The success of copper(I) tert-butyl-imino-2,2-dimethylpyrrolidinate prompted the

analogous silver(I) and gold(I) compounds to be synthesized and studied as CVD

precursors for metal films. These two particular silver and gold compounds proved to be

a vast improvement compared to previously reported amidinate and guanidinate

compounds.1 The iminopyrrolidinate compounds could be evaporated and entrained into a

deposition zone without decomposing. For comparison, to obtain thin gold films from

[Au(NiPr)2CNMe2]2 the substrate is placed directly over the solid precursor.

5 The

evaporation temperatures of the precursors were sufficiently separated from their onset of

metal deposition that future ALD experiments should be attempted. Because of their low

evaporation rates an appropriate precursor delivery system may be needed. Other silver(I)

and gold(I) alkyl-imino-2,2-dimethylpyrrolidinate compounds should be studied to

discover an alternate precursor with higher rates of evaporation and higher solubility to

simplify their synthesis.

Various diamino carbenes were tested as ligands for precursors in monomeric

copper(I) hexamethyldisiliazide compounds. The carbenes investigated a range of N-

substituents and nature of the carbon backbone. Many potential precursors were

Page 227: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

204

discovered. The series of imidazolinylidene compounds demonstrated consistent volality

and thermal stability. Results for the formamidinylidene compounds were also

encouraging. Since a good understanding has been established regarding the behavior and

properties of a range of diamino carbenes it would be appropriate to expand the family of

precursors stabilized by carbenes to include other copper(I) compounds; e.g. alkoxides,

alkyl, alkylamido. A primary goal should be to reduce the steric bulk of the anionic

ligand without sacrificing stability in order to assist the reactivity of the precursor with

surfaces and reducing agents.

Initial ALD experiments employed 1,3-diisopropyl-imidazolin-2-ylidene copper

hexamethyldisilazide in a plasma-enhanced process. Self limited growth was

demonstrated at 225 °C on silicon with a native oxide. Thermal ALD experiments

involving the same precursor and molecular hydrogen were reported on Ru and Pd

substrates.6 On Ru substrates isolated nanoparticles of copper metal were deposited

between 170 – 240 °C with 1000 cycles. The density and size of the nanoparticles varied

at each temperature which indicates a variation in either precursor chemisorption or

reactivity of molecular hydrogen. On Pd substrates, film continuity was observed to be

dependent on the thickness of the underlying Pd film. Substrates with 70 nm of Pd

afforded films with a non-obvious interface between Cu and Pd as observed by TEM. A

graded interface with intermixed Cu/Pd phases was suggested. Substrates with <10 nm of

Pd afforded films similar to Ru substrates. A self-limiting growth rate of 0.45 Å/cycle

was confirmed at 220 °C. Arguably, the growth rate was stable between 190 °C and 250

°C, although a growth rate vs. temperature plot showed a steadily increasing growth rate

from 0 to 1.3 Å/cycle between 150 °C and 350 °C on thick Pd films. Considering a recent

Page 228: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

205

report describing the role of Pd films in thermal Cu ALD employing molecular

hydrogen,7 it is possible that the observed variable growth rate was an effect of variable

hydrogen uptake in Pd with temperature. A saturation curve for the hydrogen pulse or

varying the purge time preceding the hydrogen pulse would help to investigate this

possibility.

The interaction of the precursor with a copper surface was modeled with DFT

calculations and concluded that chemisorption of the precursor likely occurs through

dissociation of the Cu-NHC bond. However, the Cu-NHC bond was calculated to be very

strong at 293 kJ/mol. It is the nature of diamino carbenes to bond strongly to metal

centers, therefore it is not possible to chemically modify the carbene to ease bond

dissociation and assist precursor chemisorption. Steric factors of the carbene are

changeable and maximising access to the central copper atom by lowering the steric bulk

of the precursor is a valid direction for future work. Low temperature PE-ALD

experiments for compounds 4 – 9 in Chapter 7 involving a variety of potential

barrier/adhesion layers would contribute to the understanding and usefulness of these

precursors.

References8.2

1 Whitehorne, T. J. J.; Coyle, J. P.; Mahmood, A.; Monillas, W. H.; Yap, G. P. A.;

Barry, S. T. Eur. J. Inorg. Chem. 2011, 3240-3247.

2 Kim, T.; Yao, Y.; Coyle, J. P.; Barry, S. T.; Zaera, F. Chem. Mater. 2013, 25, 3630-

3639.

3 Wu, J.; Li, J.; Zhou, C.; Lei, X.; Gaffney, T.; Norman, J. A. T.; Li, Z.; Gordon, R.;

Cheng, H. Organometallics 2007, 26, 2803-2805.

4 Ma, Q.; Guo, H.; Gordon, R. G.; Zaera, F. Chem. Mater. 2011, 23, 3325-3334.

Page 229: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

206

5 Mandia, D. J.; Griffiths, M. B. E.; Zhou, W.; Gordon, P. G.; Albert, J.; Barry, S. T.

Physics Procedia 2013, 46, 12-20.

6 Hagen, D. J.; Povey, I. M.; Rushworth, S.; Wrench, J. S.; Keeney, L.; Schmidt, M.;

Petkov, N.; Barry, S. T.; Coyle, J. P.; Pemble, M. E. J. Mater. Chem. C 2014, 2, 9205-

9214.

7 Jiang, X.; Wang, H.; Qi, J.; Willis, B. G. J. Vac. Sci. Technol. A. 2014, 32, 041513

Page 230: Group 11 Precursors for Atomic Layer Deposition: …...Group 11 Precursors for Atomic Layer Deposition: Design and Synthesis of Advanced Precursors Enabled by Investigations in Thermolysis

207


Recommended