M. Gilchriese Glued Fittings October 5, 2005
Transcript
Page 1: M. Gilchriese Glued Fittings October 5, 2005. M. Gilchriese 2 Samples and Prep Three samples using Hysol 9396 Seven samples using Hysol 9394 Surface prep.

M. Gilchriese

Glued Fittings

October 5, 2005

Page 2: M. Gilchriese Glued Fittings October 5, 2005. M. Gilchriese 2 Samples and Prep Three samples using Hysol 9396 Seven samples using Hysol 9394 Surface prep.

M. Gilchriese2

Samples and Prep

• Three samples using Hysol 9396• Seven samples using Hysol 9394• Surface prep tubes

– Sandpaper(600) with alcohol– Wash with alcohol– Wash with acetone

• Surface prep fitting– Brass wire brush with alcohol– Wash with alcohol– Wash with acetone

• Irradiate to about 25 MRad (exact value TBD)• He leak -> P to 15.5 bar -> He leak -> irradiate -> P to 15.5 bar

-> He leak

Page 3: M. Gilchriese Glued Fittings October 5, 2005. M. Gilchriese 2 Samples and Prep Three samples using Hysol 9396 Seven samples using Hysol 9394 Surface prep.

M. Gilchriese3

Samples After Irradiation• Note that epoxy turns blue-like color. No evidence of epoxy running.

Page 4: M. Gilchriese Glued Fittings October 5, 2005. M. Gilchriese 2 Samples and Prep Three samples using Hysol 9396 Seven samples using Hysol 9394 Surface prep.

M. Gilchriese4

Before/After Comparison

• Small weight gain

• Note that did not try to control electrical contact between fittings and pipe. Resistance after. Did not measure before.

• Change in leak rate not significant. Small change from setup on different days.

SampleWeight Before

Weight After(10/4) After-Before

Resistance After

Leak Before Leak After

96A 1.9813 1.9838 0.0025 Open 1.10E-09 1.30E-0996B 1.9788 1.982 0.0032 Open 1.10E-09 1.30E-0996C 1.97 1.9735 0.0035 0 1.20E-09 1.30E-0994A 1.8542 1.8579 0.0037 Open 1.10E-09 1.40E-0994B 2.0056 2.0073 0.0017 Open 1.10E-09 1.20E-0994C 1.8837 1.8855 0.0018 0 1.10E-09 1.30E-0994D 1.7724 1.7748 0.0024 Open 1.20E-09 1.60E-0994E 1.7756 1.7778 0.0022 0 1.10E-09 1.50E-0994F 1.7809 1.7833 0.0024 0 1.00E-09 1.10E-0994G 1.9228 1.9256 0.0028 Open 1.30E-09 1.50E-09

Page 5: M. Gilchriese Glued Fittings October 5, 2005. M. Gilchriese 2 Samples and Prep Three samples using Hysol 9396 Seven samples using Hysol 9394 Surface prep.

M. Gilchriese5

9396 Pictures

Page 6: M. Gilchriese Glued Fittings October 5, 2005. M. Gilchriese 2 Samples and Prep Three samples using Hysol 9396 Seven samples using Hysol 9394 Surface prep.

M. Gilchriese6

9394 Pictures

Page 7: M. Gilchriese Glued Fittings October 5, 2005. M. Gilchriese 2 Samples and Prep Three samples using Hysol 9396 Seven samples using Hysol 9394 Surface prep.

M. Gilchriese7

Cross Section 9396

9396

Tube in aboutCorrect Longitudinalposition

Page 8: M. Gilchriese Glued Fittings October 5, 2005. M. Gilchriese 2 Samples and Prep Three samples using Hysol 9396 Seven samples using Hysol 9394 Surface prep.

M. Gilchriese8

Cross Section 9394

9394

Tube notFullyInserted

Big void

Glue film

Page 9: M. Gilchriese Glued Fittings October 5, 2005. M. Gilchriese 2 Samples and Prep Three samples using Hysol 9396 Seven samples using Hysol 9394 Surface prep.

M. Gilchriese9

First Conclusion

• Promising but need more testing

• Thermal cycling about to start

• Will do pressure cycling also

• Mechanical strength tests to follow, need to define protocol

• Need more tests in C3F8 not irradiated and irradiated to understand penetration into epoxy. Bulk epoxy samples

• Assuming all is OK, better control of glue application and assembly. These samples were done in a hurry.