NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT,...

Date post: 12-Aug-2020
Category:
Upload: others
View: 1 times
Download: 0 times
Share this document with a friend
41
Warren C. Oliver 1 & George M. Pharr 2 2 University of Tennessee, Dept. of Materials Science and Engineering; & Oak Ridge National Laboratory, Materials Science & Technology Division Knoxville, TN Research sponsored in part by the Division of Materials Sciences and Engineering, Office of Basic Energy Sciences, U.S. Department of Energy, and by the National Science Foundation, and the Alexander von Humboldt Foundation. NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, AND FUTURE 1 Nanomechanics Inc., Oak Ridge, TN Nanomechanics Inc
Transcript
Page 1: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …mech.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura... · Warren C. Oliver 1 & George M. Pharr 2 2 University of Tennessee,

Warren C. Oliver 1 & George M. Pharr 2

2 University of Tennessee, Dept. of Materials Science and Engineering; &

Oak Ridge National Laboratory, Materials Science & Technology Division

Knoxville, TN

• Research sponsored in part by the Division of Materials Sciences and Engineering, Office of Basic Energy Sciences,

U.S. Department of Energy, and by the National Science Foundation, and the Alexander von Humboldt Foundation.

NANOINDENTATION IN MATERIALS RESEARCH:

PAST, PRESENT, AND FUTURE

1 Nanomechanics Inc., Oak Ridge, TN

Nanomechanics

Inc

Page 2: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …mech.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura... · Warren C. Oliver 1 & George M. Pharr 2 2 University of Tennessee,

OUTLINE

A Brief History

• the instrument (WCO)

• the method for H&E measurement (GMP)

• the obvious applications (GMP)

Some Applications That Weren’t So Obvious

• geology & planetary materials (WCO)

• polymers & viscoelastic materials (WCO)

• the continuum to atomistic bridge (GMP)

• biology & medical science (WCO)

• some unusual applications (GMP)

Page 3: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …mech.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura... · Warren C. Oliver 1 & George M. Pharr 2 2 University of Tennessee,

THE ORIGINAL

NANOINDENTER

Page 4: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …mech.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura... · Warren C. Oliver 1 & George M. Pharr 2 2 University of Tennessee,

THE ORIGINAL NANOINDENTER

• Pethica, Hutchings, and Oliver, Phil Mag A48, 593(1983)

Page 5: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …mech.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura... · Warren C. Oliver 1 & George M. Pharr 2 2 University of Tennessee,

BASIC MEASUREMENTS

65.3°

Berkovich indenter

1 mm

Page 6: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …mech.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura... · Warren C. Oliver 1 & George M. Pharr 2 2 University of Tennessee,

• Pethica, Hutchings and Oliver,

Nuclear Instruments and Methods,

209/210 (1983)

THE ORIGINAL APPLICATION

• Hardness of ion-implanted metals

Page 7: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …mech.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura... · Warren C. Oliver 1 & George M. Pharr 2 2 University of Tennessee,

THE METHOD:

A BRIEF OVERVIEW

Page 8: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …mech.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura... · Warren C. Oliver 1 & George M. Pharr 2 2 University of Tennessee,

KEY PRIOR WORK

N.A. Stillwell & D. Tabor

“Elastic recovery of conical indentations”Proc. Phys. Soc. London 78, 169 (1961)

I.N. Sneddon

“The relation between load and penetration in the axisymmetric

Boussinesq problem for a punch of arbitrary profile” Int. J. Engng. Sci. 3, 47 (1965)

S.I. Bulychev et al.

“Determination of Young’s modulus according to indentation

diagram”Zavod. Lab. 41, 1137 (1975)

J.L. Loubet et al.

“Vickers indentation curves of magnesium oxide (MgO)” J. Tribology 106, 43 (1984)

M.F. Doerner & W.D. Nix

“A method for interpreting the data from depth-sensing indentation

instruments”JMR 1, 601 (1986)

Page 9: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …mech.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura... · Warren C. Oliver 1 & George M. Pharr 2 2 University of Tennessee,

THE FUNDAMENTAL EQUATION

Sneddon, Int J Engrg Sci 3, 47 (1965)

P

hc

ha A

z

r

z = f(x) ; x=r/a

• Pharr, Brotzen, & Oliver, J Mater Res 7, 613 (1992)

P(a)2Eeffax2f'(x)dx

1 x20

1

; Eeff E

1 2

h(a)f'(x)dx

1 x20

1

hc lim2

x2

1yf(y)dy

(y2 x2) 1 y20

1

x 1

S dP

dh 2Eeffa

2

Eeff A

Page 10: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …mech.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura... · Warren C. Oliver 1 & George M. Pharr 2 2 University of Tennessee,

HARDNESS & MODULUS MEASUREMENT

Eeff E

1 2

S

2a

2

S

A

H P

A

A A(hc )

hc hmax Pmax

S(area function)

• Oliver & Pharr, J Mater Res 7, 1564 (1992)

P

h

S=dP/dh

hmax

Pmax

loading

unloading

9.4 mm

65.3°

Berkovich indenter

Page 11: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …mech.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura... · Warren C. Oliver 1 & George M. Pharr 2 2 University of Tennessee,

MONOLITHIC MATERIALS

Page 12: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …mech.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura... · Warren C. Oliver 1 & George M. Pharr 2 2 University of Tennessee,

ASSESSMENT OF METHOD

0

50

100

150

200

250

300

350

400

0 50 100 150 200 250 300 350 400

Nominal valueCuMgMoStainless steelSnTiamorphous SiO2brass

Nan

oin

den

tation

Mo

du

lus,

E (

GP

a)

Conventional Modulus, E (GPa)

Page 13: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …mech.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura... · Warren C. Oliver 1 & George M. Pharr 2 2 University of Tennessee,

OBVIOUS APPLICATIONS

• Surface modified materials

- ion implanted

- laser treated

- radiation damaged

• Thin films

-semiconductor

- magnetic storage

- optical coatings

• Materials of limited size

- powders

- small crystals

• Composite & multiphase materials

• Hard coatings

- machine tool

- thermal spray

- diamond-like carbon (DLC)

• Weldments & joints

9.4 mm

Page 14: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …mech.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura... · Warren C. Oliver 1 & George M. Pharr 2 2 University of Tennessee,

GEOLOGY & PLANETARY

MATERIALS

Page 15: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …mech.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura... · Warren C. Oliver 1 & George M. Pharr 2 2 University of Tennessee,

• Chakoumakos, Oliver, Lumpkin and Ewing, Radiation Effects and

Defects in Solids, 118 (1991)

LONG TERM RADIATION DAMAGE

Page 16: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …mech.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura... · Warren C. Oliver 1 & George M. Pharr 2 2 University of Tennessee,

-10

-9

-8

-7

-6

-5

-4

-3

0

2

4

6

8

10

12

14

16

0 50 100 150 200 250

Hard

nes

s (G

Pa)

Position (microns)

Log D

ose

(10

15

Alp

has/

mg)

Chakoumakos, Oliver, Lumpkin and Ewing, Radiation Effects and

Defects in Solids, 118 (1991)

RADIATION DAMAGED ZIRCON

Page 17: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …mech.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura... · Warren C. Oliver 1 & George M. Pharr 2 2 University of Tennessee,

POLYMERS &

VISCOELASTIC MATERIALS

Page 18: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …mech.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura... · Warren C. Oliver 1 & George M. Pharr 2 2 University of Tennessee,

CONTIUOUS STIFFNESS MEASUREMENT

Elastic

-2

-1

0

1

2

-1

-0.5

0

0.5

1

0 10 20 30 40 50

Exc

itatio

n fo

rce

(µN

)

Response displacem

ent (nm)

Time (milliseconds)

Viscoelastic

-2

-1

0

1

2

-1

-0.5

0

0.5

1

0 10 20 30 40 50

Exc

itatio

n fo

rce

(µN

)

Response displacem

ent (nm)

Time (milliseconds)

= 0°

= 90°

• Oliver & Pethica, US Patent No. 4,848,141, July 1989

Page 19: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …mech.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura... · Warren C. Oliver 1 & George M. Pharr 2 2 University of Tennessee,

Courtesy of Tom Fleischman and Remi Granier, Goodyear Tire & Rubber Co.

45 µm dia. flat punch; 10 Hz

AUTOMOTIVE TIRES

Page 20: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …mech.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura... · Warren C. Oliver 1 & George M. Pharr 2 2 University of Tennessee,

NANOIMPRINT FORMING

Nanometer gap polymer

squeeze flow, 115 °C

• Courtesy of Graham Cross, CRANN, Trinity College Dublin

Page 21: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …mech.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura... · Warren C. Oliver 1 & George M. Pharr 2 2 University of Tennessee,

THE CONTINUUM TO

ATOMISTIC BRIDGE

Page 22: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …mech.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura... · Warren C. Oliver 1 & George M. Pharr 2 2 University of Tennessee,

GETTING “BETWEEN” THE DISLOCATIONS

P

highly stressed zone

L 1

m-2 101210131014

L mm1.00.30.1 • Shim et al, Scripta Mater 59, 1095 (2008)

Page 23: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …mech.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura... · Warren C. Oliver 1 & George M. Pharr 2 2 University of Tennessee,

POP-IN & THE THEORETICAL STRENGTH

• Page, Oliver, and McHargue J Mater Res 7, 450 (1992)

Hertzian AnalysisP

aR

0.48a45°

h

At pop-in:

max theo G / 30G / 5

e.g.: Al2O3, W, Ni3Al, Au,

Cu, Al, Ni, Mo5SiB2,

CaF2, etc.

max 0.31pm 0.316PEr

2

3R 2

1/ 3

80 nm 350 nm

Berkovich

(001) sapphire

pop-in

Displacement, h (nm)

Load, P

(m

N)

65.3°

0 100 200 300

30

20

10

0

Displacement, h (nm)

loading

unloading

Load, P

(m

N)

0 20 40 60 80

8

6

4

2

0

Page 24: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …mech.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura... · Warren C. Oliver 1 & George M. Pharr 2 2 University of Tennessee,

ATOMISTIC MODELING

• courtesy Prof. A. Hartmaier,

Ruhr University Bochum

P

(111) copper single crystal

2.5x106 atoms; (30 nm)3

R = 8 nm; h = 2 nm

Molecular Dynamics Simulation

Page 25: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …mech.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura... · Warren C. Oliver 1 & George M. Pharr 2 2 University of Tennessee,

THE INDENTATION SIZE EFFECT

P1

A1

P2 > P1

A2

Hardness:

H P

A

Smaller is stronger !

Ma & Clarke, J Mater Res. 10, 853 (1995)

Single Crystal Silver

conventional plasticity

Berkovich

65.3°

Page 26: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …mech.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura... · Warren C. Oliver 1 & George M. Pharr 2 2 University of Tennessee,

BIOLOGY &

MEDICAL SCIENCE

Page 27: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …mech.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura... · Warren C. Oliver 1 & George M. Pharr 2 2 University of Tennessee,

CORTICAL vs. TRABECULAR BONE

Interstitial lamellae

Cortical(dense, compact)

osteon

Transverse section

trabecular struts

Trabecular(spongy, cancellous)

• Turner et al, J Biomech 32, 437 (1999)

transverse section

trabecular

bone

cortical bone

osteon

10-500 mm

Specimen E (GPa)

Acoustic

E (GPa)

Nanoindentation

trabecular 17.2 18.2 ± 0.5

cortical (transverse) 15.1 16.6 ± 0.3

cortical (longitudinal) 20.9 23.4 ± 0.6

Page 28: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …mech.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura... · Warren C. Oliver 1 & George M. Pharr 2 2 University of Tennessee,

WOOD CELL WALLS

cellulosic

microfibrils

• Konnerth et al, J Mater Sci 44, 4399 (2009)

Page 29: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …mech.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura... · Warren C. Oliver 1 & George M. Pharr 2 2 University of Tennessee,

SOME UNUSUAL

APPLICATIONS

Page 30: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …mech.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura... · Warren C. Oliver 1 & George M. Pharr 2 2 University of Tennessee,

HYDROTHERMAL VENT GASTROPODS

• Yao et al, PNAS 107, 987 (2010)

“Protection mechanisms of the iron-plated armor of a deep-sea hydrothermal vent gastropod”

Page 31: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …mech.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura... · Warren C. Oliver 1 & George M. Pharr 2 2 University of Tennessee,

HYDROTHERMAL VENT GASTROPODS

• Yao et al, PNAS 107, 987 (2010)

“Protection mechanisms of the iron-plated armor of a deep-sea hydrothermal vent gastropod”

C. Squamiferum (2001)

Page 32: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …mech.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura... · Warren C. Oliver 1 & George M. Pharr 2 2 University of Tennessee,

HYDROTHERMAL VENT GASTROPODS

• Yao et al, PNAS 107, 987 (2010)

“Protection mechanisms of the iron-plated armor of a deep-sea hydrothermal vent gastropod”

C. Squamiferum (2001) Vent crab

Page 33: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …mech.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura... · Warren C. Oliver 1 & George M. Pharr 2 2 University of Tennessee,

HYDROTHERMAL VENT GASTROPODS

• Yao et al, PNAS 107, 987 (2010)

“Protection mechanisms of the iron-plated armor of a deep-sea hydrothermal vent gastropod”

C. Squamiferum (2001) Vent crab

Page 34: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …mech.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura... · Warren C. Oliver 1 & George M. Pharr 2 2 University of Tennessee,

HYDROTHERMAL VENT GASTROPODS

• Yao et al, PNAS 107, 987 (2010)

“Protection mechanisms of the iron-plated armor of a deep-sea hydrothermal vent gastropod”

Armor Mechanics (FEM)

OL: Fe-based granular

• tough

• abrades penetrator

ML: organic

• compliant

• arrests cracks

• protects brittle ILIl: calcified shell

• structural support

• fatigue/bendiing resistance

C. Squamiferum (2001) Vent crab

Page 35: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …mech.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura... · Warren C. Oliver 1 & George M. Pharr 2 2 University of Tennessee,

THE LAACHER SEE HYPOTHESIS

• Riede & Wheeler, J Archaeological Sci 36, 2384 (2009)

“Testing the „Laacher See hypothesis‟: tephra as dental abrasive”

Page 36: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …mech.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura... · Warren C. Oliver 1 & George M. Pharr 2 2 University of Tennessee,

THE LAACHER SEE HYPOTHESIS

• Riede & Wheeler, J Archaeological Sci 36, 2384 (2009)

“Testing the „Laacher See hypothesis‟: tephra as dental abrasive”

Page 37: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …mech.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura... · Warren C. Oliver 1 & George M. Pharr 2 2 University of Tennessee,

THE LAACHER SEE HYPOTHESIS

• Riede & Wheeler, J Archaeological Sci 36, 2384 (2009)

“Testing the „Laacher See hypothesis‟: tephra as dental abrasive”

~11,000 BC

Page 38: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …mech.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura... · Warren C. Oliver 1 & George M. Pharr 2 2 University of Tennessee,

THE LAACHER SEE HYPOTHESIS

• Riede & Wheeler, J Archaeological Sci 36, 2384 (2009)

“Testing the „Laacher See hypothesis‟: tephra as dental abrasive”

~11,000 BC

Page 39: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …mech.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura... · Warren C. Oliver 1 & George M. Pharr 2 2 University of Tennessee,

TESTING THE HYPOTHESIS

red deer tooth

Er

dentinenamel

H

Hard

ne

ss, H

(G

Pa

)

Mo

du

lus. E

r(G

Pa

)

Location (mm)

Hardness (GPa)

Hardness

Particle

Ash

Page 40: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …mech.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura... · Warren C. Oliver 1 & George M. Pharr 2 2 University of Tennessee,

TESTING THE HYPOTHESIS

red deer tooth

Er

dentinenamel

H

Hard

ne

ss, H

(G

Pa

)

Mo

du

lus. E

r(G

Pa

)

Location (mm)

Hardness (GPa)

Hardness

Particle

Ash

Page 41: NANOINDENTATION IN MATERIALS RESEARCH: PAST, PRESENT, …mech.fsv.cvut.cz/~nemecek/teaching/dmpo/literatura... · Warren C. Oliver 1 & George M. Pharr 2 2 University of Tennessee,

Thanks for your attention !!