NBSIR 73-103
Stress Corrosion Behavior of High
Strength Corrosion Resistant Materials
E. Escatante and W. F. Gerhold
Corrosion Section
National Bureau of Standards
Washington, D. C. 20234
February 7, 1973
Prepared for
Materials Division
Naval Air Systems CommandDepartment of the Navy
NBSIR 73-103
STRESS CORROSION BEHAVIOR OF HIGH
STRENGTH CORROSION RESISTANT MATERIALS
E. Escalante and W. F. Gerhold
Corrosion Section
Metallurgy Division
February 7, 1973
Prepared for
Materials Division
Naval Air Systems Command
Department of the Navy
U. S. DEPARTMENT OF COMMERCE, Frederick B. Dent, Secretary
NATIONAL BUREAU OF STANDARDS, Richard W. Roberts, Director
Progress Report
on
Stress Corrosion Behavior of High StrengthCorrosion Resistant Materials
E. Escalante and W. F. GerholdCorrosion Section
Metallurgy Division
Results to date in the investigation of the stress -corrosion behaviorof high strength corrosion resistant materials (authorized under RRMA 2007)are included herein.
The materials that are being studied in this investigation includethe following:
Alloy Steels
PH 14-4 Mo, "C "-ringsPH 14-8 Mo, sheet17-4 PH, sheet17-4 PH, forgingPH 15-7 Mo, sheetAM 350, sheetAM 355, sheetAM 355, wireAM 357, sheet17-7 PH, sheet17-7 PH, wireThermenol , sheetA 286, sheetHNM, sheet17 Cr-5 Ni, foilCustom 450Custom 455
Titanium Alloys
6 A1-4VC105 VAA110 ATCI 15 VAB120 VCA
The tests are being conducted in the marine atmosphere at the SO' and
800' lots at Kure Beach, North Carolina. Table 1 and Table 2 contain the
results obtained from tests conducted at the 80' and the 800' lots, respec-
tively.
These tests are continuing.
—
'
a>CC} ?Hf-i cd -H
2
r--
r—2 »
i—t o>«t LO LOr-^ (Ni
ct! ^ca, cd
PC u. tu2 2 Z 2o. f*.
r-» r---
/—\ /—\ v£> —
I
•-—1 ^—' O tOH
CN]
o00
/—
\
00 MDO v—
'
r—I •>+J 2 oo 1
CD r-» m3to tO CN1 tOX 3 PC » p-.ti.y-i U-, P., v
—
y -\
aj rH 2 2 2 2 2 2 2 CNJ LOa -h /— /—> 00 /—-s /—-\ /—
\
/—v /—\ r—\ LOcd tO N H M K) to to to sD totu v t v / ^
[ 1—1 *rj" r-» r-. to Lf) (N N CM CO (M H 00 CNJ (NJN O O)
ooO MO toto LO
to 00 tJ-(NJ ttJ- V.O
r-l r-t 00 I—
I
CNJ 00 r—4 tOr-l rH CNJ COE-1 co
0 >Hfn
3co OOPho\°XUJ
LO o oN O) O LO o or-~ o LO o or~-~ ct> o O LO o oCO N CTl O O LO O OLn n oi o
+->
CD
S+->
ct5
CD
fn
*3
cc!
•Hr-t
CD+->
CC5
CO00G•H Ph tufn o cro oo oy a> o
4->
I—
I
_+-)
o aj r
CD T3rH CD
CD !hCD
rH ItCD
X E- CDH
Ph
oo
+->
ccj :
3CD
rHCD
CD
H
o oLO LOo orH Z - - rH
RH
CO
3
> -h< Q CTJ
XI X) X> XJ X> X) X X X X X X X .£> vO Ci (N
O ^+->
—
i
CO
CO
- \DMD i—
(
" /—
*
•> LO tOCO i—< v—
'
LO - LO"> , ^ i—l
O M •>(M ^—' tO ^
*» LO r—( LOCT) « -> v—
'
•-h
tn
CT>o lo r~- o lo n c oCD >i i—l I—I r-i I—I i-Hu3 4h(/) ooXPJ
o oMP d)a uu w 3>,r-H
> cd -H< a cdPU
4-1
o ^MV) Jh
c3 i—
i
a -hctf
PU
Xl Tt M Nv >
i—i -
rH
re *3-ai tj-CM •>
t-l CMi—I «to a>CM i—
I
00 00LO CN!
Ln cm
CM CM
CM i-H
CM \£>CM i-i
O 00 OXI CM CM 00v_>tO *>r-t»o o
a» to i-tto •> •>r-H /—\ CT>i—t '—' *O CTl OI—t I—i \01 *y
00 vOCM r-H CM
^ tOX> *tf rQ
to x—
'
CMcr>
CM
CTl
CTl
CM 00tO 00
•> i—
i
o -LO CM•n- en
1—1 00CM LO
/—
\£) vO(O H H H rj- CM LO
CDCO Jh
ct$ 1-hQ -HPL,
vD /T-> rHlO CM rt CM
>—' * tOrs CM fx /—\ /—
\
o LOCM CM LO CM CM oo i—
1
v ' * •> V J *
—
J i—l
LO O 00 H 00 L/l i—l CMCM CM rH tJ- CM CM o Ol
o> •» •\ «\ CM rH O00 /"~\ /""N to 00 /—v I—
V
r—l
I—
1
vO tO LO \ 1 tO tO CM CM to f—
\
I—
1
to -> v / v > to to to toto LO vD vO 'it LO 00 00 LO LO v > 1—
'
CM tO H H H rH CM i—( i—l r-H i—
i
00 1—1 to to to
+Jcoo
0rH
a
•H -H
cd tu
CO T3CD
O
o
oPh> CJ> CM OOr-^ i—i rt- loLO tO 00 r-Hi-i h o torH rH CM CM
O CM tO toto to to to
\0 tO CM
to to to to
to to to to
tJ- kO to 00
CD CD to CT>Is- h i/i CM tO CO T00 CM VD
to
to
a>
uH->
coCO
CD
rH
to
oPL,o\°
XUJ
cwo
O LO o oLO N Ol O O LO o olo cd o oLO LO o oo o O LO o olo r-~ cr> o O
LO o otO Mj) O
+->
c(1)
£+J
cd
fHH
ct3
rHCD
Mcci
s
+->
CDCD
rCto
o1—
I
rH
oLOto
o +-> cd
^ « 3CD X rH> CTJ -H< Q 03
4hO ^+->
/»->> r~> '—s /—
v
in to lo lov > V I \ I < '
K) M "t
CT\ LO to CMCM
CO
CM
toCM LO
•> i—I /—\ to/—> •> ^J- *>CM /—* *—' /—
s
^ to tovO *—' »> v—
'
rH tO CM CM
CM
i—\ >—\ r-> loJ3, X) N O
lo
toco
i—I i-HrH
CM CMOO CMLO i-HCM >« CMO O
i-H O
O « vOr- /—% ooCM CM 00
•» ^— #vvO cn ooo to to00 LO i—
I
Xi Xi X)
to
cCD
e+->
03
uE-
o3
•HrHCD+->
oj
2
CDCD PL, CD
CD O•H O
CO O o00 O LO
l LO oo r z X H - - - O CO z z z rHo CO o OS i-HrH o r-H u i-H XrH i-H 03 oi03 o CT$ o XL0 LO Cl.LO LOto to
i
< rH
LOr--o
X
tpv t
CO O04 .p CD
fn (/> 30) X rH> rt -h< Q tj
Pu
/—\ cx> ooO O) .-H 00 O 00lo \o voCM
U-, Ll,
O". r-H
NO OtO vO toi-H tO
oo, to
r-H "sj* CMO r-H t^-\0 O HtO r-H
or-H
CM•> O
/ V cr> oo O CM
CD OMP d)^ to 3CD X rH> rt -h< Q cd
\0 N CiCl M 00
lo
LO /—"v CM 00rQ Tf I—
I
to r-ito .aLO v—
'
X J i
LO/—
\
CTi/—
V
rHv—' CM CM r-l
O v—
'
Tf ^^ vD+-» vQ LO to LO
CD VO 00 tO LO to TfV) ^ tO r-l "tO •> Tf to TfX 3 rH lo CM •> LO \£> i CMCti pH •> i—l c% Tf to r-»Q -H O •> CT> 00 CT>
c 00 tO r-lrH Tf rH 00 * to to
•t «fc «k - to •» '—
'
CT> o LO Ci^ M Ol LO Tf LO VO vO o> rH TfM vO \£> i—l i—( to Tf to rH tO
to
co cd
to
o
T3
O CtJ
cdtp toO O
ft• XO B32
3
tO tO CM
tO tO CM
LO Tf LO Tf
LO LO LO LO
tO rH Tf CM
Tf Tf Tf Tf
O O O OLO LO LO LO
o o o oLO LO LO LO
o too VI
v >
1c
rH pCO Tf CM Tf 00 Tf vO cr> cn Tf 00 Tf Tf v£> LO CO
CD •H1—1
3
oo3,o\°Xw
O LO om N O LO o olo r-~ o O LO o o1/1 N CJl O O LO O Olo r*- cn o o LO o oin n o o
4->
CD
6Pce
CD
Sh
H
C3
CD
PaJ
uI
Xc_5
i
a>
u
O -rH PrH CCtS O
oCu
i
oCM
+-> CD
CO GOCD CTj
to1—
1
+->
CD
CD ai CD -a +j>> C X CD CDo U •H to +-> CDi—
i
CD Cfi
rH 3 = = = totO P ?Hc •H o pH bO 1—1
o rH C rH c ofi H O a O rHa> rJ •iH i—
1
e vO +-> ctSu 00 3o CM i-H
< So
oLOto
CD o00 +J CD0$ fn?-< co 30) X r-l> rt -h V CD r-l r-l
•» CN vD >—' » *\0 '—
'
CN1 tO CMr-l o /—
^
CM i—l i-H•> r-l
£!>to « tO CM \0r-l tO to i-H rH 1—1
t/>
CD CD
e•H -Ho rtCD Vu
CO T3CD
4-1 CO
O Ou*
o tu52
to to to
to to to
to to to
to to to
O o oLO ^ LO
O o oLO ^ LO
o o o oLO LO LO LO
o o o oLO LO LO L0
o coo CO
N '
1C
1—1ol
CD •Hi—l CD in
X> U r*cU
E-
Expos
00 o ^ tO LO toi—I O "3- LO Oi"vl" rH LO lo to r-.i—l CM CM i—l CM CM
O O 00\o cn rf00 CM LO
Ol Ol 00
o>O \D CD
vO tO O (M OO C ^
00 to LO t**o "5t
oo to lo r*.
CO
CO
OU ••M COCO • O LO O OLOO OlOO OloO OLOOO O LO o o
lo n w Lor^cn m n en w n o> lo cn o lo a> oCD >- i—I i-Huco OoOho\=>Xm
+>
CD
ep0
H
CcS
as
•Hf-i
CD+->
2
o
O
LOI
uu
13CD
as :
U
oo
oLO
eoCO
u
ooo
<co
>-Sfr
<
0 O60 P 005 Sh
f-l (O 30 x ^> CO -H< a R)
Pc
^3 XI 43 X> X) X> X> Xl X)
tpo wP
0)
to Jh
co i—
i
a -hco
CO
c *oo 06 «"H•H >HO co0 PCft\CO 13
0)tpo
CO
oft
pj
o o o oLO LO LO LO
o o o oLO LO LO LO
o o o oLO LO LO LO
po coo tov—/
co0 •H1—1 a) to
X) f-l ^CO 3
to
o
B*PJ
to
co
Vf-i
•
4-> COco
0 >1P3
vO 00 i—
I
CM tOCM
vO LO CMoo cm i—i r^-
O0 M Cl N00 to LO c
—
O LO o oLO N ffi O O LO o oLf) h- 0~1 O O LO o ol/l N CD O
P0epco
0
E-
Cco
co
•HP. >
o£ ^ o LO o
1—
1
1—1 CM•H I I—
1
1—1 i—l
CO < 03p•HE-
oX!co
to
cd
Tj
tHO
p0
pto '7-; CM
P co
PLO to
CM 0t—
<
pa> i—i O
£j I l o
pp P P
P p 0
>c C o•H •H •H £
0i—l r—
1
Pi—l i—
1
i
—
1 ft•H •H •H •HP P P 0 f-l 010 to to bO cJ5 £
rf •HCO to to O
13 O 00 0 0 P ft£ s £ CO P coH •H •H oo O O p XI0 0 0 C 0a, ft ft 0 e pco to to £ 3P i—iP. f-l f-l co to HO o o 0 13 co4-1
CD O CDW) P 5h03 3
m hCD X-H> o3 oi< Q B.
OONI
oLOtO
CM 00CM LO o
O CD to o-.4-> 5h /—
\
CMCM I—
1
10 i-l > ' CMX'H i—
1
LO«j Cj CM to i-H
O i-HCM to
v '
00 or-H CM •3-
CD
5h
3to
O
ouCD
to cQ -H
o5h
CD U•l-l
5h
o3
S
•r-l
P5h
O2
to
CD H>
CD PL,
CO 13CD
to 5h CD cop 5-1 5-i •Ht-H O CD COa 5h ^410
CD to co
0i CO +-) oCD o &5-1 XP 0JCO oo
COCMp to
CD o3 to
rH CDiJD 5h •
oJ P COH co
CD >h
3
0) O 0)
> aj cti< Q [i
CMCM
o in
aj
t- )0S
o to LO Ol vO vO o a--!—
1
to CM Or-l to 1—
1
O 00 LO CMr-H 1—
(
r-l 1—1 r-H i—
t
totO
UPCO
CO
>-
V) OOX
LO LO LO LO LO LO1^-
LO LO1^-
LO
+-> +->
c a>o p oe 0)p Q> to PCS
a> o ©60 P f-i«J 3f-l W r-l© x-h> rt< u.
o ©p f-iW rH
Q b
13
•Ho3
©ft-CO 13
0)
O
o2
Oft
to
oLf)
oLO
oLO
oLO
oLO
po tou to
COco
© >-fn
t/) Oofto\°X111
pcsca
H
C
•Hf-l
0)
P03
2
lo1^
LO LO
P©(0
10
o
s3•Hc
P
<
>i
i—
i
<
<CO
LOo
CM LOto to CM to CMi—
i
I—
1
i—
1
T—
1
i—i
i—I C7>
P P p10 to to
© © ©p P p
C c•H •H •H
i—l i—l T—
1
7—1 i—
(
1—1
•H •H •HP P P
LO LO tO V) in
tO tO to
c a© © ©s e sH •H •H -ao O o o© © © 60ft ft ft aj10 10 to ©
DOfn f-l f-i
o O o © am ip
to a) to © P
o O o 3LO o ft ft ft © r—
1
i—l CM X X X •H Oi—l i—( w w 0J Cm COu 03
oj o ©
form NBS-114A H--71)
U.S. DEPT. OF COMM. I 1. PUBLICATION OR REPORT NO. 2. Gov't AccessionBIBLIOGRAPHIC DATA
j NBSIR 73-103N°'
3. Recipient's Accession No.
4. TITLE AND SUBTITLE
Progress Report on Stress Corrosion Behavior of HighStrength Corrosion Resistant Materials
5. Publication Date
January
6. Performing Organization Code
7. AUTHOR(S) _ _ . , „. _ _ i . ,E. Escalante and W. F. Gerhold
8. Performing Organ i/.mon
9. PERFORMING ORGANIZATION NAME AND ADDRESS
NATIONAL BUREAU OF STANDARDSUtrAKlMtlNl Ur LL/MMllK^E.WASHINGTON, D.C. 20234
10. Hro|cct/T.isk/Work Unit No.
3120410
11. Contract/Grant No.
12. Sponsoring Organization Name and Address
Materials DivisionNaval Air Systems CommandDepartment of the Navy
13. Type of Report Si PeriodCovered
14. Sponsoring Agency Code
15. SUPPLEMENTARY NOTES
16. ABSTRACT (A 200-word or less factual summary of most significant information. If document includes a significantbibliography or literature survey, mention it here.)
This report contains results to date in the investigation of the stress-corrosionbehavior of high strength, corrosion-resistant materials exposed to marineenvironments. These materials are high strength alloy steels and titanium alloysin the form of c-rings, wire, sheet, forgings, and foil. The investigation is stillin progress.
17. KEY WORDS (Alphabetical order, separated by semicolons) Alloy Steels; high Strength materialsmarine environment; stress .corrosion; titanium alloys.
18. AVAILABILITY STATEMENT
UNLIMITED.
1x1 FOR OFFICIAL DISTRIBUTION. DO NOT RELEASETO NTIS.
19. SECURITY CLASS(THIS REPORT)
UNCL ASSIFIED
20. SECURITY CLASS(THIS PAGE)
21. NO. OF PAGES
14
22. Price
UNCLASSIFIED
USCOMM-OC 6