Testing of water penetration under pressure – NBR 10.787/94 (April 2007)Cement: CPII-E 32
Testing of water penetration under pressure – NBR 10.787/94 (April 2007)Cement: CPII-E 32
Applied water pressure:• day 1 to day 2: 0,1MPa• day 3: 0,3MPa• day 4 to day 7: 0,7MPa
cement content CPII-E 32 350kg/m³
design strength 20MPa
fine aggregate 388kg/m³
coarse aggregate 0 421kg/m³
coarse aggregate 1 632kg/m²
water 192kg/m³
plasticiser admixture 0,3% a 0,4% mc
Slump 90±10mm
W/C ratio 0,54
Penetron Admix 1% of the cement content
Testing of water penetration under pressure – NBR 10.787/94 (April 2007)Cement: CPII-E 32 - 1 week after start of water pressure
Testing of water penetration under pressure – NBR 10.787/94 (April 2007)Cement: CPII-E 32 - 2 weeks after start of water pressure
Testing of water penetration under pressure – NBR 10.787/94 (April 2007)Cement: CPII-E 32 - 3 weeks after start of water pressure
Testing of water penetration under pressure – NBR 10.787/94 (April 2007)Cement: CPII-E 32 - 4 weeks after start of water pressure