Date post: | 03-Feb-2016 |
Category: |
Documents |
Upload: | ricceballos |
View: | 29 times |
Download: | 2 times |
1
Basics in Welding and Weldability
HGRS/MTC
2"Basics in Welding and Weldability"Maintenance training
Objective
Outline the most important concepts and rules of welding in the cement industry
Create awareness around the main key success factors of high quality welding
Provide examples from the cement industry
2
3"Basics in Welding and Weldability"Maintenance training
Agenda
Welding process
Weldability of steels
Welding techniques
Welding defects
Practical examplesKiln shell crack repairHydrogen induced cracks
Conclusions
4"Basics in Welding and Weldability"Maintenance training
Welding process
The process of welding employs the heat of an external source (usually electrical arc) to bring metals to be welded to a molten state. The metals fusing takes place almost instantaneously
From this point of view, welding has many similarities with steel heat treatments, especially Quenching and this has to be taken in consideration
3
5"Basics in Welding and Weldability"Maintenance training
Welding process
. Quenching is a heat treatment which
objective is to form a very hard and resistant (but brittle) martensitestructure: The material
is heated until it reaches its austenitic
structure and then directly cooled down to
the ambient temperature
Carbon – Iron Diagram
6"Basics in Welding and Weldability"Maintenance training
Welding process
1400°C1000°C900°C600°C
200°C
3mm
In a welding process, there are 2 main operations :
1. Melting and fusing in the zone under the arc
2. Heat treatment in the area around
The higher the cooling speed is, the higher is the amount of martensite structure formed
Martensite is a very hard, resistant but brittle steel structure
Preheating is used to reduce the cooling rate (speed) after welding
Heat Affected Zone : HAZ
4
7"Basics in Welding and Weldability"Maintenance training
Welding process
8"Basics in Welding and Weldability"Maintenance training
Welding process
In general molten steels have a strong affinity for oxygen, nitrogen and hydrogen : if the welding atmosphere is not controlled, the molten metal will pick-up some oxygen or/and hydrogen, forming oxides/nitrides or/and other structures as the weld solidifies. These are impurities which will embrittlethe weld and weaken it
For this last reason shielded welding techniques (or welding under controlled atmospheres) were developed : SAW (Submerged Arc Welding), MIG (Metal Inert Gas), …
5
9"Basics in Welding and Weldability"Maintenance training
Weldability of steels
The term weldability is relative : practically all metals are weldable. Some however require special welding procedures in order to preserve the properties and characteristics designed for
The quality of welding may be affected by any one of the following factors :
OxidationNon metallic inclusionsChange of structureGas solubility of metalCoefficient of thermal expansionOperator, welding current/voltage, …
10"Basics in Welding and Weldability"Maintenance training
Classification of steels
The classification used in this document is based on the chemical composition (DIN & AFNOR), Examples from the Cement industry :
6
11"Basics in Welding and Weldability"Maintenance training
Ordinary Steels
Iron/Carbon alloys (C<1.2% in general), with small quantities of Mn (<0.8%) and Si (<0.5%) and other ‘impurities’ (S and P)
< 0.25% Carbon, there are no precautions to be taken for welding
%CTensile Strength
kg/mm2Yield Strength
kg/mm2Elongation
% Brinell Hardness
Low Carbon < 0.15 35 - 42 20 28 - 30 < 120
Mild 0.15 - 0.3 40 - 45 20 - 25 22 - 25 120 - 140
Medium Carbon 0.3 - 0.6 45- 65 22 - 35 22 - 15 140 - 180
High Carbon 0.6 - > 0.8 65 - > 85 40 - > 50 14 - 6 180 - > 220
Classification according to DIN and AFNOR (based on Chemical composition)
12"Basics in Welding and Weldability"Maintenance training
Ordinary Steels0.25 – 0.4% Carbon, Preheating is needed because the critical cooling speed which forms the martensite might be exceeded
Above 0.4% Carbon, preheating is a must. The temperature of preheating is around 75 – 350°C depending on the thickness (see low alloy steels)
For welding casehardened steels, the casehardened layer must be removed even with preheating
For quenched steels, preheating, maintaining at stable temperature during welding and slow cooling process are needed
Classification according to DIN and AFNOR (based on Chemical composition)
7
13"Basics in Welding and Weldability"Maintenance training
Low Alloy Steels
At least one alloy element is added in a quantity < 5% to improve the steel properties (Mechanical Resistance, Corrosion and Abrasion)
The Carbon content is not sufficient to predict the weldability, some alloy elements participate also in the process of martensite formation : the Carbon Equivalent % has to be considered
Minimal Content in %
Mn 1.2Ni 0.5Cr 0.25V 0.05Si 1Mo 0.1
Co, Ti, Al, Cu, W 0.3
Classification according to DIN and AFNOR (based on Chemical composition)
14"Basics in Welding and Weldability"Maintenance training
Low Alloy Steels
Actually, it is the cooling velocity around the welding seam which must be controled :
Preheating which objective is to reduce the cooling rate after weldingCovering the area welded for slow coolingIn some special cases (steels with high quenching aptitude), the cooling is controled in a furnace (50°C per hour)
8
15"Basics in Welding and Weldability"Maintenance training
Low Alloy Steels
The preheating level depends on :The material composition : Carbon equivalent (%CE)The thicknessSéférian Diagram (Thickness, %CE, preheating T°)
carbon equivalent
0
50
100
150
200
250
300
350
400
0 50 100 150thickness in mm
tem
pera
ture
in C
0.2
0.25
0.3
0.4
0.5
0.6
0.7
0.8
%CE = C+Mn/6+(Ni+Cu)/15
+(Cr+Mo+V)/5
16"Basics in Welding and Weldability"Maintenance training
High Alloy SteelsThe content of at least one alloy element exceeds 5%
The weldability of such steels has to be analyzed case by case
Maximal content in %
Ni 30Cr 30Mn 14Si 4W 20Mo 8V 5
Cu 2Al 12Co 18Ti 1.6
Classification according to DIN and AFNOR (based on Chemical composition)
9
17"Basics in Welding and Weldability"Maintenance training
High Alloy Steels
13% Mn Steels : Abrasion/Impact resistant steels very sensitive to precipitation of carbides around 250°C, the welding sequences must be controlled in order to limit the temperature increase
Application : Hardfacing of crusher hammers and impact bars
Example
18"Basics in Welding and Weldability"Maintenance training
High Alloy SteelsChromium, Molybdenum materials : Usually >1%C, 2-30% Cr, and 0-3% Mo.The carbides formed (Mainly C + Cr, 10 – 40%) are very hard and resistant but very fragile (notch effect due to carbides)
The structure of the matrix (martensite, austenite, …), and the form and dimensions of carbides depend on the heat treatment (especially the solidification speed) and has a large influence on the behavior under wear and impact
In most of the cases, welding is not recommendedor should be performed by specialized third parties
Application : liners and inlet wall for ball mills
Example
10
19"Basics in Welding and Weldability"Maintenance training
Welding techniques
The common techniques used in cement are :Manual Arc weldingSubmerged arc welding : SAWMIG/TIG
20"Basics in Welding and Weldability"Maintenance training
Manual Arc Welding
Most common technique
Deposition rate around 1.5 kg/h
Better control of post-welding deformation
Less sensitive to lack of fusion defectsThe welding electrode coating role is :
. Stabilizing the arc
. shielding the arc: prevent from
atmospheric contamination (O2, N2)
. Scavenging and deoxidizing :
produce a slag blanket to protect the
molten crater (and reduce its cooling)
11
21"Basics in Welding and Weldability"Maintenance training
For special works (I.e. kiln shell replacement), the welder must be qualified and certified according to DIN/EN 287-1, ASME9 or equivalent
Manual Arc Welding
5 -10°
22"Basics in Welding and Weldability"Maintenance training
Manual Arc Welding
The deposition rate can be increased by using more welders (place restrictions may apply)
The oscillating welding technique is unfavorable for residual stresses, the straight line technique gives better results
To avoid thermal distortions, the welding sequence must be determined carefully
12
23"Basics in Welding and Weldability"Maintenance training
For special works (i.e. kiln shell replacement), the electrodes have to be heated (dried) 2 hours at 200-350°C and must be kept at this temperature while welding
It is very important
To define and stick to
The welding
Procedure rules
Manual Arc Welding
24"Basics in Welding and Weldability"Maintenance training
Semi automatic / Automatic Arc Welding
In the semi-automatic arc welding, the electrode is mechanically fed through a welding gun into the arc from a continuously wound coil. The operation still needs an operator
In the fully automatic arc welding, the electrode is fed through welding jaws into the arc from a continuously wound coil. The welding doesn’t need an operator
These 2 techniques increase welding speed, reduce welding time and thus allow lower welding cost
13
25"Basics in Welding and Weldability"Maintenance training
Submerged Arc Welding
Very high deposition rates : 10kg/h, the welding velocity is around 80cm/mn
Semi-automated process
Very high quality of weld with
specialized operator
Wire and flux must
correspond to the material
26"Basics in Welding and Weldability"Maintenance training
Submerged Arc Welding
Commonly used for welding kiln shells external and internal
14
27"Basics in Welding and Weldability"Maintenance training
Metal Inert Gas (MIG) Welding
Semi automated process with Gas protecting the weld pool
This Welding process is sensitive to lack of side-wall fusion and cold lapping defects
Defect occurs in case of lack of gas
Certified people
Deposition rate: 2.5 kg/h
28"Basics in Welding and Weldability"Maintenance training
Welding defects
The most common welding defects are :Cold cracking, or hydrogen induced crackingSolid inclusionsPorositiesLack of fusionShape defects (design related defects)Lamellar tearingHot cracking
15
29"Basics in Welding and Weldability"Maintenance training
Hydrogen induced cracking : Cold cracking
Hydrogen induced cold cracking : occurs at low temperatures (< 150°C), usually originates from the weld toe, and it is caused by the diffusion of hydrogen from the weld deposit to embrittle the existing martensite structure
The hydrogen comes mostly from moisture associated with fluxes :
Usage of low hydrogen consumables. TIG and MIG prcessess, being fluxless, give lower levels of hydrogenUsage of austenitic electrodes (I.e. 2222) : the hydrogen diffusion rate is lower in austenite structure
30"Basics in Welding and Weldability"Maintenance training
Hydrogen induced cracking : Cold cracking
16
31"Basics in Welding and Weldability"Maintenance training
Solid inclusions
The most important is slag Inclusion which arises because it is difficult to ensure that all pockets of slag are removed from the weld surface (particularly when access is difficult). Slag deposits are produced by the welding flux
Oxide inclusions usually result from inadequate precleaning of the joint surface
32"Basics in Welding and Weldability"Maintenance training
Porosities
Porosity occurs when a weld is saturated with a particular gas (hydrogen, nitrogen, CO) which forms bubbles on discontinuities in the metal
Gases originate from air entrainment in the arc atmosphere (hydrogen, nitrogen), grease and moisture on joint faces or welding consumables (hydrogen) or chemical reaction in the weld (CO)
Factors of influence : instability of the arc, inefficient cleaning of the surface, and bad control of the arc at stops and starts
17
33"Basics in Welding and Weldability"Maintenance training
Lack of fusion and lack of penetration
The welding arc is not sufficiently ‘penetrating’ to ‘wet’ the edge, or does not completely fill the joint
Generally depend on the electrode manipulation, joint design, arc current and surface preparation
Example : shell joining section
34"Basics in Welding and Weldability"Maintenance training
Shape defects
Example : undercut, poor profile, misalignment
Consequence of poor electrode manipulation, bad fit-up, or/and incorrect procedure (current, voltage, speed, …)
Undercut is caused by too high current or too low speedToo low current can cause excessive spatter
18
35"Basics in Welding and Weldability"Maintenance training
Lamellar tearing
Development of cracks in the base metal in parallel with the seam surface : The bonding between the inclusions and the matrix in the base metal is weak and some inclusions will brittle, therefore strains in the thickness direction will cause de-cohesion and fracture of inclusions
36"Basics in Welding and Weldability"Maintenance training
Lamellar tearingPreventing measures :
Modification of welding procedure and joint design to reduce strains in the thickness direction
Usage of low inclusion levels (I.e. low sulphur steels)
Special heat treatments that modify the shape of porosities
19
37"Basics in Welding and Weldability"Maintenance training
Hot cracking
Occurs during or just after solidification below 1200°C
Due to the presence of low melting point components such as iron sulphides or phosphidewhich mechanical resistance is lowered under temperature
It is admitted to be due to shrinkage strains before cohesion
Inter-granular
38"Basics in Welding and Weldability"Maintenance training
Weld seam design
The weld design
has a direct impact
on its resistance :
Fatigue Strength
Load
cycles
20
39"Basics in Welding and Weldability"Maintenance training
Weld seam design
40"Basics in Welding and Weldability"Maintenance training
Welding Material
The most special electrodes commonly used in the cement industry are :
2222 of Castolin : kiln tires, rollersE7018 : kiln shell
21
41"Basics in Welding and Weldability"Maintenance training
Welding with 2222
Electrode that provides an optimum combination of strength and ductility
Factors to consider :Linear Coefficient of thermal expansionEffects of dilutionSigma phase precipitation
170 - 210Hardness HB40 - 45Elongation %
390Yield strength N/mm2650 - 690Tensile strength N/mm2
Eutectic 2222
42"Basics in Welding and Weldability"Maintenance training
Welding with 2222Linear Coefficient of Thermal Expansion (TEC)
The Thermal Expansion Coefficient increases with temperatureAt 300°C, the TEC of the following materials are :- Austenitic steel (stainless) : 17.2 10-6/°C- Eutectic 2222 : 14.4 10-6/°C- 0.2% Carbon steel : 13.4 10-6/°C- Chromium Iron : 10 10-6/°CThe stainless steel welding will expand and contract significantly, this will increase the residual stresseswhilst distorting the jointEutectic 2222 has a TEC very close to the Carbon steel, in operation, this results in maximum safety margin against cracks
22
43"Basics in Welding and Weldability"Maintenance training
Welding with 2222
Effect of dilutionDilution is expressed as the amount of parent metal ingressed in the weld depositWhen conventional stainless steel electrodes are used to weld carbon steels, the weld metal will inevitably be diluted with the parent metal by at least 20 – 30%, this creates a weld deposit which may be embrittled due to martensite formationThe 2222 weld is capable of ‘dissolving’ a high proportion of steel (~50%) whilst retaining its natural austenitic structureReference : Schaeffler diagram Cr equivalent vs. Ni equivalent
44"Basics in Welding and Weldability"Maintenance training
Welding with 2222
Sigma phase precipitationBrittle Iron-Chromium intermetallic which is very dependent on temperature and time kinetics. It can form at 900°C within minutes and after several days at 500°CIt often occurs when welding thick carbon steel section with with 309 or 310 based electrodesEutectic 2222, even when diluted can not reach the sigma zones and is therefore resistant to embrittlementReference : ternary diagram Nickel/Chromium/Iron
Example of application : kiln tires and rollers
23
45"Basics in Welding and Weldability"Maintenance training
Welding with E7018E7018 : American Welding Society numbering system
E : Metal arc welding electrode70 : Minimum allowable tensile strength of deposits expressed in 000 pounds / inch2
1 : All welding positions8 : arc characteristics and polarity (ac and dc)
Iron powder – low hydrogen electrode : rimmed steel core wire upon which a lime covering is applied
Yield strength: 470 MPa, Tensile strength: 540 MPa, Elongation: 30%
46"Basics in Welding and Weldability"Maintenance training
Welding with E7018
Because this covering is slightly thicker than normal, the arc is shorter and moderately penetrating, the slag is heavy and friable and the deposited metal lies in a flat bead providing a very reduced tendency for underbead cracking (cold cracking)
E7018 belongs to the Low Moisture Absorption electrodes family
24
47"Basics in Welding and Weldability"Maintenance training
Welding with E7018
Preheat is generally not required to prevent hydrogen induced cracking
Preheat should be used with hardenable steels to prevent the formation of hard heat-affected zones and eliminate tendencies toward quench cracking on cooling
Preheat may be required in welding heavy sections
Basics in Welding and weldability
Practical example 1
kiln shell crack repair
25
49"Basics in Welding and Weldability"Maintenance training
Fatigue and Crack formation
Kilns are exposed to dynamic loads : fluctuating stresses that can be bending, torsion, tensile, compression or combinations of these
Stresses like these can lead to crack formation and fracture without any kind of deformation and real overload
50"Basics in Welding and Weldability"Maintenance training
Fatigue and Crack formation
The load and stress changes are higher because of heat deformations and possible incorrect adjustment (typical case : crank in the tube)
Examples of areas where cracks can start : shell welding joints, toe of welds between shell and supports, manholes, satellite cooler supports, …
Circumferential weldsLoose tires pads
26
51"Basics in Welding and Weldability"Maintenance training
Crack repair
52"Basics in Welding and Weldability"Maintenance training
Crack repair
When a crack is detected, the first actions are :1. Finding the length of the crack2. Finding the depth of the crackThis is done with NDT
methods as UT, MP or DP
If the crack is throughgoing,
it is necessary to work from both
inside and outside
27
53"Basics in Welding and Weldability"Maintenance training
Crack repair procedure
The normal procedure is the following :1. Gouging from one side to about 2/3 of the thickness
2. The gouging must start a little away from the crack ends in sound material, gouging towards the crack, to avoid crack propagation
Crack end
Smooth transition radius
Gouging direction
54"Basics in Welding and Weldability"Maintenance training
Crack repair procedure3. Careful cleaning by grinding
4. Preheating : If the result of the Carbon equivalent is higher than 0.41 it is necessary to preheat. It must be pointed out that even if the result is lower than this, it does not harm to preheat, especially with heavy sections and if the weather is cold
28
55"Basics in Welding and Weldability"Maintenance training
Crack repair procedure5. Welding with a normal basic electrode as AWS E
7016 or E 7018 (The electrodes have to be dry)
6. Each run should be overpeenedto reduce stresses, and carefully cleaned from slags
56"Basics in Welding and Weldability"Maintenance training
Crack repair procedure7. Grinding down the surface of the weld : Root weld
8. The process has to be repeated from the other side controlling that the root is completely clean
9. Control with UT, MP and/or DP
29
57"Basics in Welding and Weldability"Maintenance training
Crack repair procedure
After the repair, in the case of long cracks, the shell can be reinforced by adding some joining plates :
Basics in Welding and Weldability
Practical example 2
Hydrogen-induced cracking - kiln shell welding
December 2003
30
59"Basics in Welding and Weldability"Maintenance training
Situation
Welding joint N°A between a 75mm thick new shell and a 60mm thick old section
Root weld and outside welding completed, internal gouging and DP done
While welding internally, a loud bang was heard : A crack was found inside the partially welded area
60"Basics in Welding and Weldability"Maintenance training
Situation
A 3.5m long crack was found in the HAZ in the old shell during the UT of the outside completed welding
The crack was not fully removed after gouging and grinding 20mm
A 1.6m long crack was also found in the partially welded groove on the inside of the kiln
MP was carried out and cracks were found also in the root weld
31
61"Basics in Welding and Weldability"Maintenance training
Investigation : External consultant
Preliminary finding was that the dye penetrantresidue was probably not fully removed
A hydrogen-induced crack (HIC) could have been developed due to welding over the DP residueA Hydrogen removal heat treatment (HRHT) should be carried out before continuing
Excess hydrogen in parent base metalMany repairs were done successfully in the pastThe joint at the other end of the 60mm thick old shell was welded to a new section without problemHypothesis not probable
62"Basics in Welding and Weldability"Maintenance training
Investigation : External consultant
HIC (or Cold cracking)
Occurs after welding has been completed
4 main Conditions :
1. Hydrogen is introduced by diffusion during the welding to the weld or HAZ :
. Moisture in the coating of the electrodes
. Oil, grease, dirt, paint, water … in the surface
. Degreasing fluids used to clean surfaces, DP or wet MP powder residues. Hydrogen in the parent metal : original casting process, heat treatment, or corrosion (example H2S)
32
63"Basics in Welding and Weldability"Maintenance training
Investigation : External consultant
2. Low preheating temperatures (<150°C)
3. Hard HAZ microstructure : Soft microstructures tolerate more hydrogen before cracking occurs. The E9018 weld metal is susceptible to HIC
4. Existence of tensile stresses on the weld seam originating from thermal contraction of the cooling or from external efforts
64"Basics in Welding and Weldability"Maintenance training
Investigation : External consultantSome indications :
1. Position and morphology : very fine and some times interrupted cracks, usually develop internally, at the toe of the adjacent weld passes and on the root weld metal
2. HIC propagate
3. More HIC develop and propagate during attempts to repair without HRHT
4. No cracking occur after the HRHT and other precautions
33
65"Basics in Welding and Weldability"Maintenance training
Investigation : Contractor
Crack only in the 60mm thick old shell
Steel : 0.24%C, 1.01%Mn, …
The crack was propagating
Cracks had not been found in any of the other kiln joints (other sections thinner !)
All cracks are hydrogen-induced and a HRHT must be carried out before any repair
It is not a standard practice to remove the DP lacquer before gouging and welding (Not acceptable statement)
66"Basics in Welding and Weldability"Maintenance training
Information from the DP supplier
The product is a paint that contains an organic resin that incorporates hydrogen in its formulation
Welding over this product must be avoided to prevent hydrogen-induced cracking
The product datasheet does not permit gouging and welding over the lacquer
34
67"Basics in Welding and Weldability"Maintenance training
RepairBefore the HRHT, for safety reasons, the contractor recommended :
Complete welding of the 3.5m long and 20mm deep groove on the externalInstallation of strong backs to prevent further cracking
HRHT : 450°C – 20 hours (december 23)
68"Basics in Welding and Weldability"Maintenance training
RepairAfter the HRHT :
In some areas the lacquer was not completely removed The 1.6m and 3.5m cracks propagated and others were created
It was reported afterwards that the contractor didn’t perform UT on the entire section : difficulty to know the history of the defects !
UT on the entire section :2 lack of fusions : 380mm and 190mm3 cracks : 35mm, 1200mm and 1500mmLaminations : 1200mm long
35
69"Basics in Welding and Weldability"Maintenance training
Repair
No additional cracks were developed after :HRHTStrict storage and handling of the E9018 welding electrodesProper cleaning of the joints before weldingRepair weldingDP was replaced by MP
70"Basics in Welding and Weldability"Maintenance training
Welding procedureWelding Procedure Specification WPS :
The ASME WPS applied by the contractor was qualified for a thickness range of 4.8mm to 56mm :- E9018-D1 electrodes (min tensile strength of 90kpsi),
preheating at 150°C, 3.2mm for the root and 5mm for the filler
The FOX EV 51 (E9018-D1) standard low hydrogen electrodes (lime covered) were used for the root and filler passes, This electrode when well prepared (backing at 300°C for 2 hours) has a diffusible hydrogen of <10ml/100g
The electrodes to be used in such applications are the special extra-low hydrogen content ESAB OK 74.78 or E7018 with a diffusible hydrogen of < 5ml/100g
36
71"Basics in Welding and Weldability"Maintenance training
Welding procedure
Welding Procedure Specification WPS :According to the hydrogen Control Method, the minimum preheating temperature should have been 180°C for diffusible hydrogen less than 9.5ml/100g to prevent HIC
The risk of HIC increased substantially when FLS replaced the low strength E7018 electrodes with the higher strength E9018-D1
72"Basics in Welding and Weldability"Maintenance training
Welding procedure
Drying and holding ovens : A temperature of 130°C was measured in the large oven that contained many electrodesThe drying and main holding oven was stored outside and directly exposed to rainIt is possible that some electrodes which were used were not baked (dried) : information from welding registers
37
73"Basics in Welding and Weldability"Maintenance training
Learning from the practical case 2
The WPS has to be prepared including all details prior to the welding
Selection of an extra low diffusible hydrogen electrode <5ml/100g : Equivalent to E7018
Preheating the shell sections at the right temperature depending on the C equivalent and thickness in all the areas between –100 and +100mm of the joint
Proper drying and storage of the electrodes has to be checked : 300 to 350°C during 2 hours
74"Basics in Welding and Weldability"Maintenance training
ConclusionsWelding is an important Maintenance activity performed in cement plants
Welding is not as simple as we imagine, special care must be given when welding alloyed materials
The welding efficiency (quality and time) impacts directly the equipment availability
The main welding parameters have to be known and prepared in advance :
Material to weld Welding technique and electrode to be usedWelding procedure : preheating temperature, cooling speed, preparation of the electrodes
38
75"Basics in Welding and Weldability"Maintenance training
Conclusions
Once developed, the Welding procedure has to be strictly followed
The contractors involved in special welding jobs must have the right experience
The NDT method to be applied has to be checked in advance
Other HGRS complementary documents :Kiln shell replacementGirth gear repair procedureMill end repair procedure