2 a) possible additional sources of error (creep test)

• temperature not constant over time• light (optical strain gages!) may be not constant• humidity (sample affected!) not constant• load or displacement may not be const.• machine/instrument creeping• creeping of strain gage• etc.

(day / night!)

Page 2: 2 a) possible additional sources of error (creep test)

2 b) Analyzing a creep experiment

0 1 2 3 4 5 6 7 80

5

10

15

20

Dis

plac

emen

t [%

]

Time [min]

secondary

tertiary

primary

Page 3: 2 a) possible additional sources of error (creep test)

0 1 2 3 4 5 6 7 80,000

0,001

0,002

0,003

0,004

0,005

Com

plia

nce

D(t)

[1/M

Pa]

Time [min]

0 1 2 3 4 5 6 7 8

1E-3

0,002

0,003

0,004

0,005

Com

plia

nce

D(t)

[1/M

Pa]

Time [min]

𝐷(𝑡)=𝜀(𝑡)𝜎 0

creep compliance

note that the values of e are given in %, so you have to divide them by 100

to evaluate creep compliance is only useful in the secondary region (marked by )D is in the range of 1/MPa

Page 4: 2 a) possible additional sources of error (creep test)

130°C 125°C 122°C 120°C 115°C 110°C 100°C 90°C

10-3 10-1 101 103 10510-6

10-5

10-4

10-3

10-2

Time (min)

Com

plia

nce

D(t)

(1/p

si)

2 c) i. time-temperature-shift for master curve at 120°C

Page 5: 2 a) possible additional sources of error (creep test)

130°C 125°C 122°C 120°C 115°C 110°C 100°C 90°C

10-3 10-1 101 103 10510-6

10-5

10-4

10-3

10-2

Time (min)

Com

plia

nce

D(t)

(1/p

si)

Page 6: 2 a) possible additional sources of error (creep test)

130°C 125°C 122°C 120°C 115°C 110°C 100°C 90°C

10-3 10-1 101 103 10510-6

10-5

10-4

10-3

10-2

Time (min)

Com

plia

nce

D(t)

(1/p

si)

Page 7: 2 a) possible additional sources of error (creep test)

130°C 125°C 122°C 120°C 115°C 110°C 100°C 90°C

10-3 10-1 101 103 10510-6

10-5

10-4

10-3

10-2

Time (min)

Com

plia

nce

D(t)

(1/p

si)

Page 8: 2 a) possible additional sources of error (creep test)

130°C 125°C 122°C 120°C 115°C 110°C 100°C 90°C

10-3 10-1 101 103 10510-6

10-5

10-4

10-3

10-2

Time (min)

Com

plia

nce

D(t)

(1/p

si)

Page 9: 2 a) possible additional sources of error (creep test)

130°C 125°C 122°C 120°C 115°C 110°C 100°C 90°C

10-3 10-1 101 103 10510-6

10-5

10-4

10-3

10-2

Time (min)

Com

plia

nce

D(t)

(1/p

si)

Page 10: 2 a) possible additional sources of error (creep test)

130°C 125°C 122°C 120°C 115°C 110°C 100°C 90°C

10-3 10-1 101 103 10510-6

10-5

10-4

10-3

10-2

Time (min)

Com

plia

nce

D(t)

(1/p

si)

Page 11: 2 a) possible additional sources of error (creep test)

130°C 125°C 122°C 120°C 115°C 110°C 100°C 90°C

10-3 10-1 101 103 10510-6

10-5

10-4

10-3

10-2

Time (min)

Com

plia

nce

D(t)

(1/p

si)

Page 12: 2 a) possible additional sources of error (creep test)

130°C 125°C 122°C 120°C 115°C 110°C 100°C 90°C

10-3 10-1 101 103 10510-6

10-5

10-4

10-3

10-2

Time (min)

Com

plia

nce

D(t)

(1/p

si)

Page 13: 2 a) possible additional sources of error (creep test)

130°C 125°C 122°C 120°C 115°C 110°C 100°C 90°C

10-3 10-1 101 103 10510-6

10-5

10-4

10-3

10-2

Time (min)

Com

plia

nce

D(t)

(1/p

si)

2 c) i. result: master curve at 120°C

master curve at 120°C

Page 14: 2 a) possible additional sources of error (creep test)

130°C 125°C 122°C 120°C 115°C 110°C 100°C 90°C

10-3 10-1 101 103 10510-6

10-5

10-4

10-3

10-2

Time (min)

Com

plia

nce

D(t)

(1/p

si)

master curve at 120°C

2 c) ii. predict compliance after 5 days

Page 15: 2 a) possible additional sources of error (creep test)

130°C 125°C 122°C 120°C 115°C 110°C 100°C 90°C

10-3 10-1 101 103 10510-6

10-5

10-4

10-3

10-2

Time (min)

Com

plia

nce

D(t)

(1/p

si)

master curve at 120°C

5 d = 5*24*60 min = 7200 min

Page 16: 2 a) possible additional sources of error (creep test)

130°C 125°C 122°C 120°C 115°C 110°C 100°C 90°C

10-3 10-1 101 103 10510-6

10-5

10-4

10-3

10-2

Time (min)

Com

plia

nce

D(t)

(1/p

si)

master curve at 120°C

5 d = 5*24*60 min = 7200 min

D(5 d) ≈ 1/psi

Page 17: 2 a) possible additional sources of error (creep test)

2 c) iii. possible prediction range at 120°C

130°C 125°C 122°C 120°C 115°C 110°C 100°C 90°C

10-3 10-1 101 103 10510-6

10-5

10-4

10-3

10-2

Time (min)

Com

plia

nce

D(t)

(1/p

si)

master curve at 120°C

Page 18: 2 a) possible additional sources of error (creep test)

130°C 125°C 122°C 120°C 115°C 110°C 100°C 90°C

10-3 10-1 101 103 10510-6

10-5

10-4

10-3

10-2

Time (min)

Com

plia

nce

D(t)

(1/p

si)

master curve at 120°C

40000 min == 0,9 months == 0,1 years

Page 19: 2 a) possible additional sources of error (creep test)

130°C 125°C 122°C 120°C 115°C 110°C 100°C 90°C

102 104 106 108 101010-6

10-5

10-4

10-3

10-2

Time (min)

Com

plia

nce

D(t)

(1/p

si)

master curve at 90°C

3e+9 min == 70000 months == 5700 years

for comparison: possible prediction range at 90°C

Page 20: 2 a) possible additional sources of error (creep test)

3. Fatigue testing

a) three examples of applications cyclic stress loading

1. wings of airplanes2. turbine blades3. rotor blades

(nicht sehr schwer, wenn zwei davon schon in b) genannt sind)

Page 21: 2 a) possible additional sources of error (creep test)

b) Wöhler curve and estimation of life time

10-1 100 101 102 103 104 105 106 107 108

20

40

60

80

100

120 Stress

Stre

ss [M

Pa]

Cycles N

Page 22: 2 a) possible additional sources of error (creep test)

b) Wöhler curve and estimation of life time

10-1 100 101 102 103 104 105 106 107 108

20

40

60

80

100

120 Stress

Stre

ss [M

Pa]

Cycles N

i. N(40 MPa) ≈ 9000 ii. N(27 MPa) ≈ 300000

i. N(40 MPa) ≈ 9000 tlife = N/f = 9000 * 1 / 0,5 s = 18000 s = = 5 hours

ii. N(27 MPa) ≈ 300000 tlife = N/f = 300000 * 1 / 1000 s = 300 s = = 5 minutes

(aim: to show that cyclic loaded components must have huge safetyfactors, if fatigue testing is not performed)