Page 1: ELECTRON BEAM WELDING PROCEDURE QUALIFICATION …€¦ · bpqr n° / reference edms no. rev. validity b-2015-01 / j3022578 1512110 0.0 approved page 3 2‐ record ebw test

EDMS NO. REV. VALIDITY

1512110 0.0 APPROVED

REFERENCE

J3022578

Date: 2015-05-08

CERN CH1211 Geneva 23 Switzerland

 

 

ELECTRON BEAM WELDING  

PROCEDURE QUALIFICATION RECORD 

WPQR (QMOB)

N° EBW‐2015‐01 

CCC CRYOSTAT 

   

 

 

 

 

DOCUMENT PREPARED BY: DOCUMENT CHECKED BY: DOCUMENT APPROVED BY:

Paula Freijedo Menendez Thierry Tardy EN/MME-FW

J. Pierre Brachet

EN-MME-FW

Gilles Favre EN-MME-FW

 

 

Page 2: ELECTRON BEAM WELDING PROCEDURE QUALIFICATION …€¦ · bpqr n° / reference edms no. rev. validity b-2015-01 / j3022578 1512110 0.0 approved page 3 2‐ record ebw test

BPQR N° / REFERENCE EDMS NO. REV. VALIDITY

B-2015-01 / J3022578 1512110 0.0 APPROVED

Page 2

 

TABLE OF CONTENTS 

GENERAL INFORMATION .............................................................................................................. 3

RECORD EBW TEST ....................................................................................................................... 3

RESULT TESTS ............................................................................................................................... 6

ANNEX (ES) ................................................................................................................................... 6  

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

Page 3: ELECTRON BEAM WELDING PROCEDURE QUALIFICATION …€¦ · bpqr n° / reference edms no. rev. validity b-2015-01 / j3022578 1512110 0.0 approved page 3 2‐ record ebw test

BPQR N° / REFERENCE EDMS NO. REV. VALIDITY

B-2015-01 / J3022578 1512110 0.0 APPROVED

Page 3

 

2‐ RECORD EBW TEST 

Equipment Type   PTR

Join type  BW

Depth of penetration  Q‐1: 1mm / Q‐1.5:1.5mm

Filler metal   N.A

Vacuum  5 x 10-4 

Welding position  PA

Other information: See p‐WPS 2015‐026‐FW & 2015‐027‐FW for welding parameters (See Annex 1) 

 

ASSEMBLY DESIGN 

Q‐1: Thickness 1mm  

Q‐1.5: Thickness 1.5mm 

 

 

 

 

 

 

 

1‐ GENERAL INFORMATION 

REFERENCE P‐WPS:  2015‐026‐FW & 2015‐027‐FW 

WELDING PROCESS:  

ELECTRON BEAM WELDING                                             

(N° 511 according to ISO 4063) 

STANDARD REFERENCE: 

ISO 15614‐11. Specification and qualification of 

welding procedures for metallic materials‐ Welding 

procedure Test‐ Electron and laser beam welding 

WELD DATE:  24 / 02 / 2015

WELDER NAME:  Thierry Tardy  ID:  ‐‐

N° SAMPLES: 2  ID. SAMPLES: Q‐1 & Q‐1.5

MANUFACTURER: CERN‐EN/MME‐FW  NOTIFIED BODY : CERN INTERNAL QUALIFICATION

BASE METALS:   

 SPECIFICATION 

/ GRADE STANDARD or REFERENCE 

GROUP

ISO/TR 

THICKNESS 

(mm) 

DIAMETER 

(mm) 

CERTIFICATE      

EN 10204 3.1      

1.  1.4429 / 316LN CERN THECNICAL 

SPECIFICATION Nº1002 8.1  1 / 1  ‐  N°1 (Annex 2) 

2.  1.4429 / 316LN CERN THECNICAL 

SPECIFICATION Nº1002 8.1  1.5 / 1.5   ‐  N°2 (Annex 2) 

Page 4: ELECTRON BEAM WELDING PROCEDURE QUALIFICATION …€¦ · bpqr n° / reference edms no. rev. validity b-2015-01 / j3022578 1512110 0.0 approved page 3 2‐ record ebw test

BPQR N° / REFERENCE EDMS NO. REV. VALIDITY

B-2015-01 / J3022578 1512110 0.0 APPROVED

Page 4

HEAT TREATMENT:  N.A 

PROCEDURE   

PREHEAT 

TEMP 

°C  PREHEAT 

TIME

  POST HEAT 

TEMP

POST HEAT 

TIME

 

PWHT MIN  °C  PWHT 

MAX 

°C  HEATING 

RATE 

°C/h COOLING RATE  °C/h

 

CLEANING : 

CLEANING METHOD BEFORE 

WELDING Degreasing  

CLEANING METHOD AFTER 

WELDING ‐ 

 

PICTURES 

 

 

 

 

 

 

 

 

 

 

 

WE CERTIFY THAT THE STATEMENT IN THIS RECORD ARE CORRECT AND THAT THE   TESTS WELDS PREPARED, WELDED AND TESTED SATISFACTORILY IN ACCORDANCE WITH THE 

REQUERIMENTS OF ISO‐15614‐11 INDICATED ABOVE  

                     

Page 5: ELECTRON BEAM WELDING PROCEDURE QUALIFICATION …€¦ · bpqr n° / reference edms no. rev. validity b-2015-01 / j3022578 1512110 0.0 approved page 3 2‐ record ebw test

BPQR N° / REFERENCE EDMS NO. REV. VALIDITY

B-2015-01 / J3022578 1512110 0.0 APPROVED

Page 5

3‐ RESULTS TEST 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

SEQUENCE TEST  STANDARD ACCEPTANCE 

CRITERIA RESULTS  REPORT N° 

VISUAL INSPECTION  ISO 17637 EN ISO 13919‐1     

Level B SATISFACTORY  ‐ 

DYE PENETRANT  ISO 3452‐1 EN ISO 13919‐1     

Level B SATISFACTORY  ‐ 

RADIOGRAPHIC 

EXAMINATION EN 17636‐2 

EN ISO 13919‐1     

Level B SATISFACTORY 

EDMS Nº1507381  

https://edms.cern.ch/document/1507381/1 

TENSILE TEST 

Tensile strength of the 

specimen shall not be lower 

than the minimum value 

specified for the application 

indicated in CERN THECNICAL 

SPECIFICATION Nº1002 Ed.5 

SATISFACTORY EDMS Nº 1502555 

https://edms.cern.ch/document/1502555/1 

METALLOGRAPHIC 

EXAMINATION EN 17639 

EN ISO 13919‐1     

Level B SATISFACTORY 

Q‐1 : EDMS N°1502555 &

https://edms5.cern.ch/document/1502555/1  

 Q ‐1.5 : EDMS Nº1505509 

https://edms5.cern.ch/document/1505509/1  

 

Page 6: ELECTRON BEAM WELDING PROCEDURE QUALIFICATION …€¦ · bpqr n° / reference edms no. rev. validity b-2015-01 / j3022578 1512110 0.0 approved page 3 2‐ record ebw test

BPQR N° / REFERENCE EDMS NO. REV. VALIDITY

B-2015-01 / J3022578 1512110 0.0 APPROVED

Page 6

4‐ ANNEX (ES) : 

ANNEX N°1: P‐WPS 

ANNEX N°2: MATERIAL CERTIFICATES 

‐ N‐1: STAINLESS‐STEEL CERTIFICATE THICKNESS 1MM 

‐ N‐2: STAINLESS‐STEEL CERTIFICATE THICKNESS 1.5MM 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

Page 7: ELECTRON BEAM WELDING PROCEDURE QUALIFICATION …€¦ · bpqr n° / reference edms no. rev. validity b-2015-01 / j3022578 1512110 0.0 approved page 3 2‐ record ebw test

Page 1 of 2  

      CERN CH‐1211 Geneva 23 Switzerland 

                     EUROPEAN ORGANIZATION                     FOR NUCLEAR RESEARCH  

1211 Geneva 23 ‐ Switzerland 

WELDING PROCEDURE SPECIFICATION – EBW 

Preliminary 

WPS No.: 2015‐026‐FW Rev.: 0 Date: 25‐02‐2015 

Operator: T. Tardy  Machine: PTR  Location: Building 100 

Ref. WPQR:   Ref. standard: ISO 15614‐11  Job No.: J3022578 

Client: Lees Andrew John  Project: CCC Cryostat 

PREPARATION 

Joint configuration:  Butt weld  Joint type: N.A.  Single/Double:  Single side 

Cleaning:  Welding position: PA  Backing: Yes 

JOINT SKETCH 

   

 

PARENT METAL(S)   Name / Grade  Standard  Group Delivery cond. Thickness (mm)  Diameter(mm)

I  316LN / 1.4429  EN 10028‐7  8.1    1  ‐ II  316LN / 1.4429  EN 10028‐7  8.1    1  ‐ 

FILLER METAL 

  Trade name  Classification  Group 

I  N.A.     

II       

WELDING PARAMETERS 

Working distance (mm):  400  HV (KV):    SW:  N.A.  Vacuum (mbar):  5 x 10‐4

  First pass  Second pass   Third pass 

Foc (mA)        1000 / 420     

Ibeam(mA)  7,5     

Welding speed(mm/s)  16,7     

Slope in (mm/°)  5mm     

Overlap (mm/°)  10°     

Slope out (mm/°)  5mm     

Deflection 

Pattern No.  1     

Frequency (Hz)  100     

Amplitude X   15     

Amplitude Y  0     

Pulsation 

Frequency (Hz):  N.A     

Duty (%):  N.A     

Mode:  N.A     

Pulse (mA):  N.A     

Ratio:  N.A     

Page 8: ELECTRON BEAM WELDING PROCEDURE QUALIFICATION …€¦ · bpqr n° / reference edms no. rev. validity b-2015-01 / j3022578 1512110 0.0 approved page 3 2‐ record ebw test

Page 2 of 2  

      CERN CH‐1211 Geneva 23 Switzerland 

TACKING PARAMETERS 

Foc (mA):      1000 / 420  Ibeam(mA):  7,5  Welding speed(mm/s):  16,7 

Slope in (mm/°):  5mm  Length (mm/°):   Slope out (mm/°):  5 

Deflection pattern No.:  1  Freq. (Hz):  Amplitude(mm)       X: 15          Y:0 

Pulsation freq. (Hz): N.A.  Duty (%):N.A.  Mode:  N.A  Pulse(mA): N.A  Ratio: N.A 

BEAM CALIBRATION 

IH (%):N.A.  ALIG X: N.A.  ALIG Y: N.A. 

UBIAS  (V): N.A.  STIG X: N.A.  STIG Y: N.A. 

HEAT TREATMENT 

Preheat temp.(°C): N.A.  Interpass temp.(°C): N.A.  PWHT procedure: N.A. 

ADDITIONAL COMMENTS 

      

ADDITIONAL INFO ENCLOSED 

 

Approved by  

Thierry Tardy 

Date  

17/03/15 

Signature 

 

Page 9: ELECTRON BEAM WELDING PROCEDURE QUALIFICATION …€¦ · bpqr n° / reference edms no. rev. validity b-2015-01 / j3022578 1512110 0.0 approved page 3 2‐ record ebw test

Page 1 of 2  

      CERN CH‐1211 Geneva 23 Switzerland 

                     EUROPEAN ORGANIZATION                     FOR NUCLEAR RESEARCH  

1211 Geneva 23 ‐ Switzerland 

WELDING PROCEDURE SPECIFICATION – EBW 

Preliminary 

WPS No.: 2015‐027‐FW Rev.: 0 Date: 25‐02‐2015 

Operator: T. Tardy  Machine: PTR  Location: Building 100 

Ref. WPQR:   Ref. standard: ISO 15614‐11  Job No.: J3022578 

Client: Lees Andrew John  Project: CCC Cryostat 

PREPARATION 

Joint configuration:  Butt weld  Joint type: N.A.  Single/Double:  Single side 

Cleaning:  Welding position: PA  Backing: Yes 

JOINT SKETCH 

 

 

 

PARENT METAL(S)   Name / Grade  Standard  Group Delivery cond. Thickness (mm)  Diameter(mm)

I  316LN / 1.4429  EN 10028‐7  8.1    1.5  ‐ II  316LN / 1.4429  EN 10028‐7  8.1    1.5  ‐ 

FILLER METAL 

  Trade name  Classification  Group 

I  N.A.     

II       

WELDING PARAMETERS 

Working distance (mm):  400  HV (KV):    SW:  N.A.  Vacuum (mbar):  5 x 10‐4

  First pass  Second pass   Third pass 

Foc (mA)        1000 / 420     

Ibeam(mA)  9,5     

Welding speed(mm/s)  16,7     

Slope in (mm/°)  5mm     

Overlap (mm/°)  10°     

Slope out (mm/°)  5mm     

Deflection 

Pattern No.  1     

Frequency (Hz)  100     

Amplitude X   15     

Amplitude Y  0     

Pulsation 

Frequency (Hz):  N.A     

Duty (%):  N.A     

Mode:  N.A     

Pulse (mA):  N.A     

Ratio:  N.A     

Page 10: ELECTRON BEAM WELDING PROCEDURE QUALIFICATION …€¦ · bpqr n° / reference edms no. rev. validity b-2015-01 / j3022578 1512110 0.0 approved page 3 2‐ record ebw test

Page 2 of 2  

      CERN CH‐1211 Geneva 23 Switzerland 

TACKING PARAMETERS 

Foc (mA):     1000 / 420  Ibeam(mA):  5  Welding speed(mm/s):  16,7 

Slope in (mm/°):  5mm  Length (mm/°):   Slope out (mm/°):  5mm 

Deflection pattern No.:  1  Freq. (Hz): 100  Amplitude(mm)       X:    15       Y:  0 

Pulsation freq. (Hz): N.A.  Duty (%):N.A.  Mode:  N.A  Pulse(mA): N.A  Ratio: N.A 

BEAM CALIBRATION 

IH (%):N.A.  ALIG X: N.A.  ALIG Y: N.A. 

UBIAS  (V): N.A.  STIG X: N.A.  STIG Y: N.A. 

HEAT TREATMENT 

Preheat temp.(°C): N.A.  Interpass temp.(°C): N.A.  PWHT procedure: N.A. 

ADDITIONAL COMMENTS 

      

ADDITIONAL INFO ENCLOSED 

 

Approved by  

Thierry Tardy 

Date  

17/03/15 

Signature 

 

Page 11: ELECTRON BEAM WELDING PROCEDURE QUALIFICATION …€¦ · bpqr n° / reference edms no. rev. validity b-2015-01 / j3022578 1512110 0.0 approved page 3 2‐ record ebw test
pfreijed
Typewritten Text
N-1
Page 12: ELECTRON BEAM WELDING PROCEDURE QUALIFICATION …€¦ · bpqr n° / reference edms no. rev. validity b-2015-01 / j3022578 1512110 0.0 approved page 3 2‐ record ebw test
pfreijed
Typewritten Text
N-2
Page 13: ELECTRON BEAM WELDING PROCEDURE QUALIFICATION …€¦ · bpqr n° / reference edms no. rev. validity b-2015-01 / j3022578 1512110 0.0 approved page 3 2‐ record ebw test
Page 14: ELECTRON BEAM WELDING PROCEDURE QUALIFICATION …€¦ · bpqr n° / reference edms no. rev. validity b-2015-01 / j3022578 1512110 0.0 approved page 3 2‐ record ebw test
Page 15: ELECTRON BEAM WELDING PROCEDURE QUALIFICATION …€¦ · bpqr n° / reference edms no. rev. validity b-2015-01 / j3022578 1512110 0.0 approved page 3 2‐ record ebw test
Page 16: ELECTRON BEAM WELDING PROCEDURE QUALIFICATION …€¦ · bpqr n° / reference edms no. rev. validity b-2015-01 / j3022578 1512110 0.0 approved page 3 2‐ record ebw test
Page 17: ELECTRON BEAM WELDING PROCEDURE QUALIFICATION …€¦ · bpqr n° / reference edms no. rev. validity b-2015-01 / j3022578 1512110 0.0 approved page 3 2‐ record ebw test
Page 18: ELECTRON BEAM WELDING PROCEDURE QUALIFICATION …€¦ · bpqr n° / reference edms no. rev. validity b-2015-01 / j3022578 1512110 0.0 approved page 3 2‐ record ebw test

Top Related