+ All Categories
Transcript
Page 1: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 1/257

Page 2: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 2/257

Page 3: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 3/257

Page 4: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 4/257

Page 5: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 5/257

Page 6: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 6/257

Page 7: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 7/257

Page 8: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 8/257

Page 9: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 9/257

Page 10: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 10/257

Page 11: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 11/257

Page 12: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 12/257

Page 13: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 13/257

Page 14: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 14/257

Page 15: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 15/257

Page 16: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 16/257

Page 17: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 17/257

Page 18: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 18/257

Page 19: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 19/257

Page 20: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 20/257

Page 21: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 21/257

Page 22: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 22/257

Page 23: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 23/257

Page 24: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 24/257

Page 25: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 25/257

Page 26: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 26/257

Page 27: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 27/257

Page 28: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 28/257

Page 29: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 29/257

Page 30: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 30/257

Page 31: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 31/257

Page 32: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 32/257

Page 33: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 33/257

Page 34: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 34/257

Page 35: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 35/257

Page 36: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 36/257

Page 37: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 37/257

Page 38: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 38/257

Page 39: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 39/257

Page 40: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 40/257

Page 41: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 41/257

Page 42: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 42/257

Page 43: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 43/257

Page 44: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 44/257

Page 45: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 45/257

Page 46: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 46/257

Page 47: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 47/257

Page 48: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 48/257

Page 49: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 49/257

Page 50: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 50/257

Page 51: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 51/257

Page 52: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 52/257

Page 53: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 53/257

Page 54: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 54/257

Page 55: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 55/257

Page 56: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 56/257

Page 57: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 57/257

Page 58: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 58/257

Page 59: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 59/257

Page 60: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 60/257

Page 61: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 61/257

Page 62: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 62/257

Page 63: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 63/257

Page 64: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 64/257

Page 65: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 65/257

Page 66: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 66/257

Page 67: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 67/257

Page 68: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 68/257

Page 69: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 69/257

Page 70: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 70/257

Page 71: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 71/257

Page 72: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 72/257

Page 73: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 73/257

Page 74: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 74/257

Page 75: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 75/257

Page 76: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 76/257

Page 77: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 77/257

Page 78: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 78/257

Page 79: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 79/257

Page 80: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 80/257

Page 81: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 81/257

Page 82: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 82/257

Page 83: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 83/257

Page 84: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 84/257

Page 85: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 85/257

Page 86: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 86/257

Page 87: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 87/257

Page 88: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 88/257

Page 89: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 89/257

Page 90: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 90/257

Page 91: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 91/257

Page 92: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 92/257

Page 93: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 93/257

Page 94: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 94/257

Page 95: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 95/257

Page 96: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 96/257

Page 97: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 97/257

Page 98: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 98/257

Page 99: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 99/257

Page 100: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 100/257

Page 101: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 101/257

Page 102: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 102/257

Page 103: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 103/257

Page 104: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 104/257

Page 105: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 105/257

Page 106: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 106/257

Page 107: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 107/257

Page 108: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 108/257

Page 109: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 109/257

Page 110: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 110/257

Page 111: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 111/257

Page 112: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 112/257

Page 113: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 113/257

Page 114: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 114/257

Page 115: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 115/257

Page 116: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 116/257

Page 117: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 117/257

Page 118: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 118/257

Page 119: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 119/257

Page 120: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 120/257

Page 121: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 121/257

Page 122: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 122/257

Page 123: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 123/257

Page 124: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 124/257

Page 125: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 125/257

Page 126: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 126/257

Page 127: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 127/257

Page 128: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 128/257

Page 129: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 129/257

Page 130: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 130/257

Page 131: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 131/257

Page 132: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 132/257

WWW.WELD.4T.COM

Page 133: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 133/257

Page 134: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 134/257

Page 135: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 135/257

Page 136: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 136/257

Page 137: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 137/257

Page 138: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 138/257

Page 139: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 139/257

Page 140: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 140/257

Page 141: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 141/257

Page 142: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 142/257

Page 143: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 143/257

Page 144: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 144/257

Page 145: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 145/257

Page 146: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 146/257

Page 147: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 147/257

Page 148: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 148/257

Page 149: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 149/257

Page 150: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 150/257

Page 151: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 151/257

Page 152: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 152/257

Page 153: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 153/257

Page 154: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 154/257

Page 155: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 155/257

Page 156: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 156/257

Page 157: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 157/257

Page 158: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 158/257

Page 159: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 159/257

Page 160: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 160/257

Page 161: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 161/257

Page 162: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 162/257

Page 163: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 163/257

Page 164: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 164/257

Page 165: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 165/257

Page 166: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 166/257

Page 167: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 167/257

Page 168: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 168/257

Page 169: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 169/257

Page 170: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 170/257

Page 171: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 171/257

Page 172: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 172/257

Page 173: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 173/257

Page 174: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 174/257

Page 175: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 175/257

Page 176: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 176/257

Page 177: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 177/257

Page 178: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 178/257

Page 179: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 179/257

Page 180: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 180/257

Page 181: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 181/257

Page 182: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 182/257

Page 183: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 183/257

Page 184: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 184/257

Page 185: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 185/257

Page 186: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 186/257

Page 187: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 187/257

Page 188: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 188/257

Page 189: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 189/257

Page 190: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 190/257

Page 191: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 191/257

Page 192: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 192/257

Page 193: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 193/257

Page 194: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 194/257

Page 195: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 195/257

Page 196: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 196/257

Page 197: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 197/257

Page 198: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 198/257

Page 199: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 199/257

Page 200: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 200/257

Page 201: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 201/257

Page 202: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 202/257

Page 203: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 203/257

Page 204: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 204/257

Page 205: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 205/257

Page 206: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 206/257

Page 207: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 207/257

Page 208: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 208/257

Page 209: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 209/257

Page 210: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 210/257

Page 211: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 211/257

Page 212: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 212/257

Page 213: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 213/257

Page 214: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 214/257

Page 215: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 215/257

Page 216: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 216/257

Page 217: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 217/257

Page 218: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 218/257

Page 219: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 219/257

Page 220: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 220/257

Page 221: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 221/257

Page 222: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 222/257

Page 223: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 223/257

Page 224: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 224/257

Page 225: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 225/257

Page 226: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 226/257

Page 227: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 227/257

Page 228: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 228/257

Page 229: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 229/257

Page 230: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 230/257

Page 231: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 231/257

Page 232: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 232/257

Page 233: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 233/257

Page 234: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 234/257

Page 235: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 235/257

Page 236: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 236/257

Page 237: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 237/257

Page 238: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 238/257

Page 239: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 239/257

Page 240: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 240/257

Page 241: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 241/257

Page 242: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 242/257

Page 243: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 243/257

Page 244: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 244/257

Page 245: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 245/257

Page 246: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 246/257

Page 247: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 247/257

Page 248: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 248/257

Page 249: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 249/257

Page 250: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 250/257

Page 251: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 251/257

Page 252: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 252/257

Page 253: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 253/257

Page 254: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 254/257

Page 255: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 255/257

Page 256: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 256/257

WWW.WELD.4T.COM

Page 257: Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

7/31/2019 Pipe Welding Procedures_2nd Ed_Hoobasar Rampaul

http://slidepdf.com/reader/full/pipe-welding-procedures2nd-edhoobasar-rampaul 257/257


Top Related