Post on 13-Apr-2018
transcript
7/26/2019 Dr. Dirk Duddeck_surface Analysis
1/12
available worldwide. Norhern Ialy alone probably
has a hundred micro-enerprises ha manuacure
implans, primarily or regional deniss. Bu even
hough only a acion, namely 120, o all he implan
sysems available in Europe could be included in his
sudy, hese represen he mos imporan brands or
major suppliers o implans.
Background and objectives
Tere is commonly a significan discrepancy beween
he responsibiliy reamen providers mus assume
or he maerials hey use vis-a-vis heir paiens andheir knowledge regarding he qualiy o hese ma-
erials as confirmed by neural and scienific sources.
As saed in he inerim repor in he previous issue,
Denal implans are an inegral par o he herapeu-
ic armamenarium o conemporary denal prac-
ices. Wih heir excellen success raes, hey have
become he globally esablished reamen aler-
naive o purely prosheic soluions or ooh loss.
And wih he variey o implan sysems offered,
i has become ever more difficul or he denis o
choose jus he righ sysem or his or her pracice
and paiens. Specific surace opographies, maerial
properies ha promoe osseoinegraion or surace
reamens are oen emphasized in adverising as
significan advanages o disinguish a given sysemom is many compeiors. According o he Asso-
ciaion o German Denal Manuacurers (VDDI), more
han 1,300 differen implan sysems are currenly
Final report of the BDIZ EDI implant study 2014/15
SEM surace analyses o120 serile-packed implans
DR DIRK DUDDECK1,2, DR HASSAN MAGHAIREH3, DR FRANZJOSEF FABER4AND DR JRG NEUGEBAUER1,5
EDI Journal 1/2015 conained an inerim repor presening he resuls or 65 implan sysems om he 2014/15
BDIZ EDI implan sudy. Tis inerim repor had ocused on noable analyical resuls or ianium implans and
on he presenaion o various surace srucures o popular implan sysems in ianium and is alloys [1]. Te
presen repor now also presens implans made o zirconia, analum and PEEK. Now ha his sudy has been
compleed, a oal o 120 differen sysems om 83 suppliers in 16 counries have been examined by scanning
elecron microscopy, doubling he number o implan sysems analyzed by he BDIZ EDI Qualiy and Research
Commitee since he firs sudy in 2008 [2,3]. In cooperaion wih he Universiy o Cologne, exensive maerial
conras images were obained and qualiaive and quaniaive elemenal analyses perormed on each o he
implans examined, using he same sudy proocol.
1 Inerdisciplinary Policlinic or Oral Surgery and ImplanologyDeparmen o Oral and Maxilloacial Plasic SurgeryUniversiy o Cologne
Direcor: Proessor Joachim E. Zller Kerpener Srae 32 50937 Kln Germany2Medical Maerials Research Insiue Berlin Klingsorsrae 116 12203 Berlin Germany3Clinical eaching Fellow, Universiy o Mancheser Implan Reerral Pracice Leeds, UK 9 Woodhouse Square Leeds LS3
1AD England4Cenre or Denisry and Oral and Maxilloacial Surgery, Universiy o Cologne, Maerials Science/Denal Maerials Research
Kerpener Srae 32 50931 Kln Germany5Denal Group Pracice Dr G. Bayer, Dr F. Kisler, Dr S. Kisler, Dr A. Elberzhagen, Dr J. Neugebauer Von-Khlmann-Srae 1 86899 Landsberg am Lech Germany
CLINICAL SCIENCE
1
7/26/2019 Dr. Dirk Duddeck_surface Analysis
2/12
CE marks do no proec he marke, or raher he
paien, om subsandard qualiy in medical devices
[4]. An inernaional group headed by he Universiy
o Geneva School o Denal Medicine has embarked
on he highly commendable ques o characerize,
classif and code denal implans saring in 2010
he so-called Implan Surace Idenificaion Sandard
(ISIS) ha migh aciliae he uure inroducion o a
possible ISO sandard or denal implans [5,6].
Te surace qualiy o implans depends on a
number o differen acors. Once he ianium im-
plan blank has been CNC-machined, i is urherprocessed using differen echniques ha ulimaely
resul in he producs specific surace srucure.
Te various processes used or ianium implans
were discussed in he firs par o he repor. Vari-
ous producion processes ulimaely conribue o
produc qualiy: he producion isel, he cleaning
seps, pos-producion handling (i.e., qualiy conrol),
packaging and serilizaion processes and he pack-
aging isel.
A sriking eaure o his sudy has been he many
differen ypes o serile packaging ha someimes
go o considerable lenghs o preven any kind o
conac o he implan wih he packaging. In ac,
several implans in he sudy ha did no ea-
ure conac-ee packaging bu were delivered in
so sealed polyehylene bags exhibied various
amouns o organic conaminans or plasic residue,
depending on heir surace roughness.
As described in he inerim repor, even a well-
srucured implan surace proven in clinical prac-
ice or many years may accumulae no insignifi-
can amouns o organic conaminans or plasic
paricles hrough abrasion, unless he implan was
delivered in non-conac packaging. Tere have
been repors in he lieraure ha hese organic
conaminans are associaed wih early implanloss or wih peri-implaniis [7]. Te documened
amouns o carbon in he regions ha are already
obvious on he maerial conras images are con-
siderably higher han he minor amouns o carbon
adsorbed om ambien carbon dioxide as presen
on any ianium implan. Te more or less sophisi-
caed echnical implemenaion o he serile pack-
aging has no direc relaion o he price o he im-
plans. Bu how ar can we le manuacurers go in
heir drive o save cos i he resul is sharp-edged
cover screws ha damage, and hereby breach, he
simple serile packaging even beore hey are used
(see he ex box on serile packaging on page 75)?
In addiion o he previously presened implan
OK to use in patients but apparently not always OK to take a closer look
Te grea majoriy o manuacurers responded posiively o he requess by he Universiy o Cologne. Neverheless, somemanuacurers declared ha hey had no ineres in his sudy. No even he proclaimed ac ha he presen sudy did no
primarily emphasize he producers ineress bu raher hose o he users caused hem o reconsider.
In a ew cases, orders or implans o be used or he purposes o his sudy were no filled and delivery was reused even
hough hese implans are used by several hundred praciioners hroughou Europe (see box Appeal o readers). Especially
noeworhy was he response om one manuacurer saing ha one could no remember ever having
received requess om users or SEM images or EDX resuls. Deniss, he saemen coninued, assumed ha hese resulswere good as a mater o course. Or else hey were no ineresed in his inormaion. And even i hey were, hey would no
know how o inerpre he daa correcly anyway. Less avourable resuls could be surpassed by he compeiion; and even
good resuls were no seller, because hey were no properly undersood by he reader. Tus, he risk o misinerpreaion ar
ouweighed any benefis o he sudy. All relevan inormaion and a variey o sudies on he requesed
implan sysem, hey concluded, could be downloaded om he companys websie. In ac, he websie offered no
evidence on he saey o he chromium-nickel-seel paricles ha were ound en masse in his sudy on an implan
by ha manuacurer. Unsurprisingly, hereore, he serile-packed implan analyzed in his sudy was no providedby he manuacurer.
Anoher manuacurer explicily did no wan o paricipae in he sudy, bu had hen decided o fill he order or a sample im-
plan and no o paricipae in any boycot. However, he shipmen conained an invoice and an explici noe o he effec ha
he implan was no o be named in any publicaion relaed o he presen sudy. We acknowledged ha desire, bu we did no
wan o deprive our implanological colleagues o he resuls. Because i he implans are good enough o be used in paiens,
hey should be good enough o presen in an SEM image.
Are we implanologiss really no ineresed in he qualiy o he sysems we use? Are we unable o evaluae he resuls o
his sudy? Do some manuacurers have o proec us om scienific sudies because we canno inerpre hem correclyanyway? Users will be able o answer hese quesions readily aer reading his repor.
2CLINICAL SCIENCE
7/26/2019 Dr. Dirk Duddeck_surface Analysis
3/12
levels o roughness (Figs. 1 o 16).
Te specific removal orques he orces neces-
sary o spli up he bone-implan inerace by un-
screwing he implan once osseoinegraion has ak-
en place do no differ beween zirconia implans
and ianium implans o similar roughness [9]. Oc-
casionally observed cases o los zirconia implans
sysems made o ianium and ianium alloys, im-
plans made o zirconia, analum and polyeher
eher keone (PEEK) were also sudied.
Zirconia as an implan maerial has been proven
or many years. I is probably in no way inerior o
ianium or ianium oxide in erms o is osseoin-
egraion poenial [8]. Te suraces exhibi differen
1 ISDS Meoxi (x500).
2 ISDS Meoxi
(x2,500).
3 Iviaclinical
(x500).
4 Iviaclinical
(x2,500).
5 IDenalpoin
Zeramex (x500).
6 IDenalpoin
Zeramex (x2,500).
7 IZibone Coho
(x500).
8 IZibone Coho
(x2,500).
1 2
3 4
5 6
7 8
CLINICAL SCIENCE
3
7/26/2019 Dr. Dirk Duddeck_surface Analysis
4/12
5 ianium (i-6Al-4V) a 6.7 Wm1K 1. Insering zir-
conia implans a he orques commonly used or i-
anium implans migh resul in emperaure peaks,
especially in high-densiy bone, ha could cause
hermal bone damage. In-viro sudies have shown
ha elevaed inserion orques lead o a significan
emperaure increase, especially in he firs ew mil-
may no be solely due o he surace properies o
hese implans. One possible cause o early implan
loss may be he low hermal conduciviy o zirconia.
Tus, he hermal conduciviy o ytrium-sabilized
zirconia, a approximaely 2.2 Wm1K1, is nearly
en imes lower han ha o grade 4 ianium (22
Wm1K 1) and hree imes lower han ha o grade
9 IAxis biodenal(x500).
10 I
Axis biodenal(x2,500).
11 IBreden WhieSky(x500).
12 IBreden WhieSky(x2,500).
13 IZ-Sysems Zirkolih(x500).
14 IZ-Sysems Zirkolih(x2,500).
15 INaural DenalImplans roo-ana-logue replicae madeenirely o zirconia(x500).
16 INaural DenalImplans roo-ana-logue replicae madeenirely o zirconia(x2,500).
9 10
11 12
13 14
15 16
4CLINICAL SCIENCE
7/26/2019 Dr. Dirk Duddeck_surface Analysis
5/12
Polyeher eher keone (PEEK) has more recenly
been used as a new maerial or denal implans (Fig.
19). As he maerial has only been used or denal
implans or a raher shor ime, only ew repors are
exan. In-viro rials sugges ha he mechanical
properies o PEEK migh opimize he disribuion o
masicaory orces hrough he implans surround-
ings [16,17]. Here we will have o wai or long-erm
clinical resuls. Only one implan made o PEEK was
included in he sudy; a second manuacurer had
no responded o our enquiries.
Materials and methods
A oal o 120 differen implan sysems om
83 manuacurers and 16 counries were analyzed
by scanning elecron microscopy (able 1). Te
SEM device used or he acquisiion o he surace
opography (Phenom proX, Phenom-World, Eind-
hoven, Neherlands) has a highly sensiive deec-
or or backscatered elecrons (BSE) ha aciliaes
inerences abou he composiion o he examined
maerial as he so-called maerial conras image
emerges. Elemens wih a low aomic number, i.e.
wih ewer elecrons, such as carbon or aluminiumare shown as relaively dark areas, while elemens
wih high aomic numbers such as ianium or zir-
conium appear relaively brigh.
For esing, he implans were aken ou o heir
packaging using a serile orceps and atached o
he sample holder beore being inroduced ino
he vacuum chamber. Because zirconia implans
are more easily elecrically charged han ianium
implans, a so-called charge-reducion sample
holder was used ha largely atenuaes his charg-
ing phenomenon, which would oherwise lead o
areacs.
Qualiaive and quaniaive elemenal analysis o
he implan suraces was perormed using energy-
limeres o he prepared implan sie [10].
One analum-ianium hybrid implan in his
sudy exhibied a raher paricular surace opo-
graphy. While he ianium surace o he implan
shoulder and is apical region had been blased
wih hydroxyapaie, he middle segmen o he im-
plan, markeed by he manuacurer as rabecular
meal, had a porous srucure no unlike cancellous
bone. Tis hree-dimensional srucure is based on
a glassy carbon amework compleely coaed wih
analum. Te corrosion-resisan analum [11] has
been successully used as an orhopaedic implanmaerial or many years. Now also used in denal
implans, he special surace exure is designed o
allow he ingrowh o bone cells ino he deph o
he srucure [12,13]. Te erm osseoincorporaion
has been coined in he lieraure in an atemp o
add a hird dimension o Brnemarksdefiniion o
osseoinegraion [14]. Prospecive mulicenre sud-
ies a 22 locaions in five European counries have
shown ha he clinical success raes o hybrid im-
plans made o ianium and analum were similar
o hose o pure ianium implans [15]. Te only
represenaive o his class o maerials in he currensudy was he analum-ianium hybrid implan by
Zimmer (Figs. 17 and 18).
17 I rabecular midsecion made o analum(Zimmer rabecular Meal implan, x500).
18 I Te shoulder and apex o he same im-plan are made o ianium (Zimmer rabecularMeal implan, x500).
19 I Implan made o polyeher eher keone(Champions WIN! PEEK implan, x500).
20 I3D roughness recon-
srucion (BredenWhieSKY, x2,500).
CLINICAL SCIENCE
5
7/26/2019 Dr. Dirk Duddeck_surface Analysis
6/12
each implan.
o documen he surace roughness o each o he
invesigaed implan sysems, a so-called 3D rough-
ness reconsrucion was perormed ha allows a vi-
sual comparison o he respecive surace srucures.
During he imaging process, he hree-dimensional
shape o he objec is calculaed om he brighness
disribuion in he grid o he our quadrans o he
backscatered elecron deecor (Fig. 20).
dispersive X-ray specroscopy (EDX). Here, he elec-
ron beam causes he primary elecrons emited o
inerac wih he aoms o he specimen surace,
releasing elecrons o he inner shell as secondary
elecrons. Te resuling gaps are immediaely filled
by elecrons om a higher orbial. Te difference in
energy is emited as an X-ray quanum and deeced
by a hermoelecrically cooled deecor, measuring
boh he elemenal composiions and heir con-
cenraions. An areal analysis and one or more spo
analyses (in case o irregulariies) were perormed or
Manufacturer Country
AB Israel3M Espe Germany/USA
Adin Israel
AGS Implance urkey
Alpha-Bio ec Israel
Alpha Den Unied Kingdom
Alphaech
(Henry Schein)
Germany
Anhogyr France
Argon Medical Germany
Avinen Spain
Axis biodenal Swizerland
Bego Germany
Bio3 Germany
Biodena Swizerland
Biohorizons USA
Biome 3i USA
Bioek BK Ialy
BlueSkyBio USA
Breden Germany
BI Spain
C-ech Ialy
Camlog Germany/
Swizerland
Champions Germany
Clinical House Swizerland
Corex Israel
Cumdene Germany
DENAL RAIO Germany
Denalpoin Swizerland
Manufacturer Country
Denaus Loser Sweden
Denaurum Germany
Denegris Germany
Denium Korea
Densply Implans Sweden/Germany
Dio Korea
FairImplan Germany
General Implans Germany
Glidewell USA
Hi-ec Israel
IDI France
Implan Direc Swizerland
ImplanSwiss Swizerland
JDenal Care Ialy
JMP Germany
Keysone USA
Klockner Andorra
KSI Bauer Germany
Lasak Czechia
m+k Germany
Medenika Germany
Medenis Germany
Medical Insinc Germany
Megagen Korea
MIS Israel
Naural Denal
Implans
Germany
Naure Implans Germany
Manufacturer Country
NBM Swizerland
Neoss Unied Kingdom
Nobel Biocare Sweden
Nucleoss urkey
OCO Biomedical USA
Ossem Korea
O medical Germany
Palop Israel
Phibo Spain
Phoenix Germany
Prowial Germany
Schz Germany
SDS/Meoxi Swizerland
SGS Hungary
SIC Swizerland
Souhern Souh Aica
Sraumann Swizerland
Sweden Marina Ialy
A-Denal Germany
Tommen Swizerland
RI Swizerland
rinon Germany
VI-SOM Ialy
viaclinical Germany
Z-Sysems Swizerland
Zibone/Coho aiwan
Zimmer USA
ZL-Microden Germany
Table 1: List of implant manufacturers participating in the 2014/15 implant study (as per 30 April 2015)
An updaed lis o all invesigaed implans and comprehensive repors on individual implans (upo hree repors per reques) are available o BDIZ EDI members by conacing he associaion office(office@bdizedi.org).
6CLINICAL SCIENCE
7/26/2019 Dr. Dirk Duddeck_surface Analysis
7/12
ac wih he packaging could be responsible.
Some isolaed implans exhibied inorganic resi-
due om he sandblasing process, namely alumina
paricles 20 o 30 m in size (Fig. 25), bu in quani-
ies o presumably limied clinical relevance.
Unexpeced inorganic residue findings included,in addiion o he iron-copper-chromium paricles
described in he firs par o he repor, larger areas
wih inermiten chromium-nickel-seel paricles 4
o 30 m in size on one o he implans sudied. Te
maerial conras image had already presened hem
as srikingly brigh and well-defined srucures. Tese
meallic paricles migh have originaed as impuriies
wihin he blasing maerial or as abrasion residue
om he CNC cuting ools ha were subsequenly
embedded in he implan surace o he poin where
cleaning could no remove hem (Figs. 26 and 27).
Tree spo analyses were carried ou as par o he
qualiaive and quaniaive elemenal analysis (Fig.
28). Te analysis o he chromium-nickel-seel paricle
Results
Minor amouns o carbonaceous residue remaining
on he implan aer he cleaning process are a no
inequen finding. Organic residue appears darker
in he maerial conras image han ianium or zir-
conia because carbon aoms have ewer elecronsand hereore creae ewer backscatered elecrons
in a SEM han aoms o higher aomic numbers. So,
someimes jagged edges are ypical o organic con-
aminans. I here are only a ew isolaed spos like
ha, hey will make up only a very small par o he
oal area, being o litle consequence and no clinical
relevance (Fig. 21). Te figure shows a single organic
impuriy 10 o 20 m in size on an oherwise largely
residue-ee implan. More conspicuous were sys-
emaically disribued organic residues on several
implans ha are in conac wih heir ouer packag-
ing. Tese ypically eaured circumerenial organic
conaminaion occurring only a he ouer edge o
he hread (Figs. 22 o 24), which suggess ha con-
21 I Single spo, individual organic conaminan (x2,500). 22 I Circumerenial organic residue on aianium implan (x500).
23 I Organic residue on he ouer hreadsrucures (zirconia, x500).
24 I Superficial organic paricles(zirconia, x500).
25 I Individual inclusions o sandblasingmaerial (ianium, x2,500).
CLINICAL SCIENCE
7
7/26/2019 Dr. Dirk Duddeck_surface Analysis
8/12
he wo paricles (spo no. 4) shows only he ypical
signs or grade 5 ianium (ianium, aluminium and
vanadium) (Fig. 31 and able 4).
Te so-called EDX mapping assigns each elemen-
(spo no. 2) has ypical fingerprins or he elemens
iron, nickel and chromium (Fig. 29 and able 2). As
expeced, he dark paricle urns ou o be alumina
(Fig. 30 and able 3), while he conrol area ouside
26 I Implan surace (Adin ouareg) wihnoable ligh and dark paricles (x500).
27 I Same implan surace (Adin ouareg):brigh chromium-nickel-iron paricle, darkaluminium oxide paricle (x2,500).
28 I Marks or EDX spo analysis andEDX mapping area (Adin ouareg; x2,500).
29 I Qualiaive elemenal analysis, spo no. 2 (brigh chromium-nickel-iron paricle).
30 I Qualiaive elemenal analysis, spo no. 3 (brigh aluminium oxideparicle; sandblasing residue).
31 I Qualiaive elemenal analysis, spo no. 4 (paricle-ee implansurace, grade 5 ianium).
able 2 I Quaniaive elemenal analysis Elemen disribuion,spo no. 2.
Aomic percenage Cerainy
Fe 49.8% 0.99
i 24.5% 0.99
Cr 13.6% 0.99
Al 5.6% 0.97
Ni 5.2% 0.96
V 1.3% 0.94
able 3 I Quaniaive elemenal analysis Elemen disribuion,spo no. 3.
Aomic percenage Cerainy
O 68.2% 0.99
Al 25.3% 1.00
i 6.1% 0.99
V 0.4% 0.93
able 4 I Quaniaive elemenal analysis Elemen disribuion,spo no. 4.
Aomic percenage Cerainy
i 85.7% 1.00
Al 11.5% 0.99
V 2.8% 0.94
8CLINICAL SCIENCE
7/26/2019 Dr. Dirk Duddeck_surface Analysis
9/12
plans exhibied no significan conaminaion. By
way o example, he suraces o ianium implans
by some manuacurers (Alpha-Bio, Argon Medical,
Avinen, C-ech, Denium, Nucleoss, Ossem, Ph-
ibo, SGS and Breden) are presened a comparable
al signal is own colour, which can hen be super-
imposed on he SEM image as a coloured overlay.
Figure 32 shows he deeced chromium in green
and aluminium in blue.
Forunaely, he vas majoriy o he sudied im-
37 I Denium Superline (x2,500).
38 I Nucleoss 4 Implan (x2,500). 39 I Ossem S III ( x2,500).
35 I Avinen Ocean (x2,500).
32 I Example o EDX mapping: green = chrome;blue = aluminium (Adin ouareg; x2,500).
33 I AlphaBio SPI Spiral Implan (x2,500).
36 I C-ech Esheic Line (x2,500).
34 I Argon Medical K3Pro Sure (x2,500).
40 I Phibo Aurea (x2,500).
CLINICAL SCIENCE
9
7/26/2019 Dr. Dirk Duddeck_surface Analysis
10/12
wih specially conduced sudies.
Up o a poin, biocompaible aluminium oxide res-
idues are unlikely o affec he bone-implan conac
(BIC) [18,19]. Bu how does he human body handle
polyehylene or chromium-nickel-seel paricles?
Even i hese paricles are relaively firmly atachedo he implan surace, hey are likely o become de-
ached by he resuling icional orces in he bone
bed as he implans are insered a orques in he
double digis o achieve he desired level o primary
sabiliy.
Paricles wih a diameer o less han 10 m are
suscepible o upake by macrophages hrough
phagocyosis [20], so ha quesions relaed o he
clinical relevance o such impuriies canno simply
be brushed aside. From orhopaedics i is known
ha paricle-induced macrophage acivaion is as-
sociaed wih an increased oseoclasogenesis and
may hereore cause increased bone resorpion [21].
One poin o criicism ha has been repeaedly
magnificaion in Figures 33 o 42. Te coninuous
improvemen process in Camlog implans deserves
special menion. While he samples analyzed in 2008
showed residues o blasing maerial on up o en
per cen o he oal surace, he figure or 2011 was
less han hree per cen or he same implan ype. Inhe curren sudy, all hree implan models (Camlog,
Conelog and iSy) exhibied compleely residue-ee
suraces in he elemenal analysis. Tus, he spec-
rum o he EDX analysis o he Conelog implan sur-
ace indicaes only ianium (Figs. 43 o 45).
Discussion
Te clinical relevance o minuscule paricles and
conaminans on denal implans is a mater o de-
bae. Even he manuacurers o implans on whose
implans more or less large amouns o organic or
inorganic conaminans were ound in ess have
repored saisical success raes ha are no differ-
en om hose o oher implans, proving heir poin
41 I SGS Pi (x2,500). 42 I Breden BlueSky ( x2,500). 43 I Camlog Conelog ( x500).
44 I Camlog Conelog, EDX area analysis (x2,500). 45 I Quaniaive and qualiaive elemenal analysis o he CamlogConelog implan surace (pure ianium).
Aomic percenage Cerainy
i 100.0% 1.00
10CLINICAL SCIENCE
7/26/2019 Dr. Dirk Duddeck_surface Analysis
11/12
medical devices where unlike wih general echni-
cal goods deecs canno be remedied or repaired
once insered. Each o he implans examined was
serile-packed and inended or use in paiens.
One migh hereore couner by asking why he
manuacurers qualiy managemen is obviously
expressed by some manuacurers in he conex o
specimen used in his sudy paterns are only ran-
dom samples. A scienific sudy requires a leas five
o seven implans o each implan ype o make sa-
isically valid saemens abou a qualiy sandard.
Bu he reply can only be ha hose implans are
Limitations o SEM resolution Or: How clean would you like it?
Te scope o elemenal analysis by energy-dispersive X-ray specroscopy (EDX) as used in his sudy is limied because i
does no deec superficial conaminaions on he nanoscale. As he elecron beam impacs he implan, i is scatered in he
sample, so ha he emited X-rays orm a pear-shaped volume having a diameer o 0.1 o 2 m. Tus, signals originaing in
he op ew nanomeres o an implan surace are exinguished by deeper signals.
Only X-ray phooelecron specroscopy (XPS) can produce such sensiive evidence in layers 5 o 10 nm in hickness.
Te kineic energy o he phooelecrons o an aom is measured o deermine is binding energy, which is characerisic o he
aom om which he elecron emanaes. Tis can be used o deermine wheher he cleaning process afer acid eching o he
implan surace has lef races o acid or i he waer used or he cleaning isel was clean enough.
An Israeli manuacurer (Palop) has decided o consisenly clean heir producs wih ulra-pure waer (UPW), whichis raher expensive o produce compared o regular demineralized waer and is oherwise mosly employed by he
semiconducor indusry.XPS analyses o he implan suraces hus cleaned show no races o sulphur, silicon, zinc orchlorine, inorganic impuriies no inequenly ound in he XPS analyses o he sandblased and acid-eched suraces o
implans by oher manuacurers invesigaed in 2014 as he corresponding ISIS idenificaion cards were prepared [22]. Te
maerial conras image showed no residue on he i-6AL-4V ELI implan (Figs. 46 and 47). Te corresponding EDX analysis
shows only he ypical elemens or grade 5 ianium (Fig. 48 and able 5).
46 I Palop Advanced Denal Implan (x500). 47 I Palop Advanced Denal Implan ( x5,000).
48 I EDX specrum or he Palop implan. able 5 I Quaniaive elemenal analysis o he i-6Al-4V ELIimplan surace (Palop).
Aomic percenage Cerainy
i 65.6% 1.00
O 24.4% 0.96
Al 7.3% 0.99
V 2.7% 0.96
CLINICAL SCIENCE
11
7/26/2019 Dr. Dirk Duddeck_surface Analysis
12/12
subjec o daily flucuaions and why implans are
released which yield subopimal resuls in individual
esing.Each day we are asked wih winning he rus o
our paiens, and each ime we perorm an implano-
logical reamen we are rying o prove worhy o his
rus. For individual manuacurers o rejec sudies like
he presen one or o allege image manipulaion is no
paricularly helpul in his endeavour. Bu he vas ma-
joriy o he sudied implans presens an encouraging
picure. By ar mos manuacurers are aware o heir
responsibiliy and provide implanologiss in Europe
wih solidly made sysems.
o find he lis o reerences visi he web (www.eam-work-media.de).Follow he link Lieraurverzeichnis in he le sidebar.
Sterile packaging bedchamber o implants:fom simple and non-sterile to elaborately protected
49 I Example o elaborae serile
packaging, longiudinal secion
(Palop).
50 I Serile packaging compromised by asharp-edged cover screw (BlueSkyBio).
While a limied number o echnologies has now akenover he manuacuring o implans, he ingenuiy o
manuacurers in packaging heir implans apparenly
knows no limis. Te sudied implans represened a wide
variey o designs, where aspecs such as ease o use, sae
ranspor, conaminaion-ee sorage and producion
coss appeared o be in compeiion.
On he one hand, here are uncompromising elaborae
consrucions ha offer sae handling and are sure o
ea ino he manuacurers profi margin (Fig. 49).Te
illusraion shows a complex packaging design where he
implan is insered in a separae sleeve made o he same
maerial (grade 5 ianium) as he implan isel o reduce
he influence o oher maerials o a minimum.
On he oher hand, here are simple packaging soluions
where he implan is simply sealed in a double plasic
bag and he manuacurer seems o have deemed even a
sabilizing ouer wrapper such as a bliser pack o be oocosly. Figure 50 shows a serile package compromised by
a sharp-edged cover screw.
Appeal o readers
We would have liked o be able o presen resulsor implans by he ollowing manuacurers:
Ihde Denal (Swizerland)
MozoGrau (Spain)
SHINHUNG (Korea)
Egar Implans (Israel) Signo Vinces (Porugal/Brazil)
Despie several reminders or placemen o a regular
order, hese implans could no be analyzed.
If you are a user of implants by these manufacturers
and as interested as we are in the results, please mail
us at duddeck@bdizedi.org.
Contact address
Dr Dirk DuddeckInerdisciplinary Policlinic or Oral Surgery andImplanologyDeparmen o Oral and Maxilloacial Plasic SurgeryUniversiy o CologneDirecor: Proessor Joachim E. Zller
Kerpener Srae 62 50937 Kln Germanydirk.duddeck@gmx.de
12CLINICAL SCIENCE